1. Introduction
Triboelectric nanogenerators (TENGs) have demonstrated the ability to convert surrounding ambient mechanical energy into electricity based on the coupling effects of contact triboelectrification and electrostatic induction. However, the need for a low-cost method and an improvement in output performance remain a challenge in TENG fabrication. A practical application to harvest mechanical energy is also required. In general, the two key factors that significantly affect the output performance of TENGs are the tribo-material and the effective contact area of the friction layers. Another study showed that the surface charge density enhanced the triboelectric material and that the surface morphologies in micro/nanopatterning control the TENGs performance [
1,
2]. As shown in 2012 by Wang’s group [
3], TENGs operate in four basic modes: vertical contact-separation mode; lateral sliding mode; single electrode mode, and freestanding triboelectric-layer mode. Among these working modes, the vertical contact–separation mode was introduced first and has become the primary mode due to its simple operation, durability, stable and high-output performance. Basically, using the electrostatic charges created on the surfaces of two dissimilar materials when they are brought into contact, the tribo-charges can generate a potential drop when two surfaces are separated by an external force and, thus, drive electron flow between two electrodes connected on both sides of the tribo-material.
Recently, TENG development has become very common in many fields, such as energy harvesting, self-powered sensors, self-charging systems, or self-powered wearable electronic devices. TENGs has been investigated to obtain higher electricity output using surface charge density enhancement via ionized injection, which alters the effective contact area between the friction tribo-layers. This improvement is through its surface patterning or through new materials developed using functional group attachment. However, the simple, low-cost, and flexible structure of TENGs through embedded nanoparticles (NPs) is still being considered as a way to increase the capacitance of TENGs. By modifying the inside polymers through filling with nanoparticles and forming pores, many studies have reported the advantages of an embedded high dielectric constant material in polydimethylsiloxane (PDMS), such as BaTiO
3, SrTiO
3 [
4,
5], Au, or Ag nanoparticles [
6], for improving TENG capacitance. In addition, the output performance of TENG can be increased by adjusting the distribution depth of the tribo-charges in the friction layer as described by Cui et al. [
7]. C. Wu et al. [
8] also demonstrated that the charge density in the friction layer is enhanced by utilizing a reduced graphene oxide (rGO) acting as electron-trapping sites [
8]. These methods can lead to the higher output performance of TENGs, but are still limited in real applications due to the complexity, high-cost, and lack of both physical characteristic and analysis properties for understanding embedded NP behaviors inside the tribo-polymers layer. Moreover, oxygen vacancies in the oxide nanoparticles are electrically positive charges [
9], which is an important factor that can contribute to the exchange and trapping of electrons when driving a TENG. In previous studies, however, the effect of oxygen vacancies within the tribo-material surface according to the oxide nanoparticle embedded ratio was not studied.
In this work, we report a significant improvement of TENG performance by considering TiO2−x NPs embedded in PDMS as a function of weight ratio. Through this work, the optimal TiO2−x NPs embedded PDMS is determined, and we investigated the correlation between TENG output behavior and the physical properties of the TiO2−x NPs-embedded PDMS, such as the surface potential, dielectric properties, oxygen vacancy, and electronic structures. Different TiO2−x NPs embedded according to PDMS weight ratios from 0 to 30% were chosen for tribo-layer fabrication. The results show a significantly enhanced TENG output upon the use of TiO2−x NPs embedded PDMS as compared to a pristine PDMS tribo-layer. The optimal TiO2−x NPs embedded PDMS with a 5% weight ratio exhibited the highest voltage of 180 V and current of 8.15 µA under a 5 N pushing force and 5 Hz pushing frequency. Furthermore, for practical applications, a portable windmill system integrated with our optimal TENGs using a low-cost, simple fabrication process involving plastic bottle waste is proposed.
3. Results and Discussion
The proposed TENG was operated using a simple model of contact–separation, as depicted in
Figure 1a. The TiO
2−x NPs-embedded PDMS layer was laminated on the Al electrode as a negative tribo-material. When the TiO
2−x NPs-embedded PDMS layer comes into contact with the top layer Al electrode (i.e., positive tribo-material) as well, the TiO
2−x NPs-embedded PDMS layer becomes negatively charged while the Al electrode is positively charged because of the different electron affinities. During the release process, potential is created between the two opposite electrostatic charges. The potential across these electrodes leads to an electron flow through the external circuit from the bottom Al electrode to the top to obtain electrical equilibrium. After full separation, the electrodes revert back to their original states, and at last, the tribo-charge distribution reaches electrical equilibrium. Applying a continuous external pushing force to the TENGs, repeated TENG operation can be observed. Since the titanium oxide materials have various physical structures, such as anatase, rutile, and bookite, and their electrical, optical, and physical properties depend on their physical structure [
10], XRD patterns of the TiO
2−x NPs were investigated, as shown in
Figure 1b. The TiO
2−x NPs represent the typical polycrystalline rutile structure with diffraction peaks of (110), (101), (200), (101), (210), (211), (220), (002), (310), (301), and (112), and the calculated particle size was about 20 nm through main XRD peak of (110). [
11,
12] The energy band diagram of the PDMS layer and TiO
2−x NPs-embedded PDMS layer with 5% and 30% are shown in
Figure 1c. As TiO
2−x NP increased, the work function difference between the two contact materials is reduced from 2.61 eV to 0.72 eV. This implies that the transport of electrons from the top Al electrode can be reduced.
Figure 1d shows the scanning electron microscope (SEM, compact SEM GENESIS-1000, Emcrafts, Korea) images of the PDMS layer and TiO
2−x NPs embedded PDMS layer with 5% and 30%. The surface morphology of these PDMS and TiO
2−x NPs-embedded PDMS layers are uniformly wrinkle-like and similar, except for the higher weight ratio TiO
2−x NPs-embedded PDMS layers. The average roughness of these TiO
2−x NPs-embedded PDMS layers is confirmed by the AFM image, and the mean surface roughness of the PDMS layer and TiO
2−x NPs-embedded PDMS layer with 5% and 30% was 17.8, 22.1, and 19.8 nm, respectively. (Not shown here).
Figure 2a,b show the output voltage and current characteristics of the TENG without/with TiO
2−x NPs as a function of weight ratio (measured under a relative humidity of ~55% and room temperature of 27 °C). As the weight ratio of TiO
2−x NPs increased from 0% (pristine PDMS) to 5%, the output voltage and current increased significantly from 112 V and 3.5 µA to 180 V and 8.15 µA, respectively. However, at weight ratios greater than 5%, the output voltage and current drastically decreased to 38.7 V and 0.6 µA, respectively. Moreover, to examine the effect of the pushing force on the output performance of the TENG device with pristine PDMS, 5% (optimal weight ratio) and 30% TiO
2−x NPs-embedded PDMS, the output voltage and current of the TENG were measured and analyzed at different pushing forces ranging from 5 to 20 N and pushing frequency of 5 Hz (
Figure S2—Supporting Information). It clearly indicates that the peak voltage and current of the TENG were increased from 48.2 V and 1.6 µA to 91.8 V and 2.9 µA for the pristine TENG, from 64.9 V and 3.8 µA to 126.8 V and 6.1 µA for 5%, and that of 30% TiO
2−x NPs-embedded PDMS based TENG increased from 30.6 V and 0.9 µA to 58.7 V and 2.1 µA by enhancing the applied pushing forces from 5 N to 20 N, respectively. The highest output voltage and current values of 126 V and 6.1 µA were obtained under the externally applied force of 20 N. This result is mainly attributed to the surface potential dramatically changing among these kind of TENGs. This was especially true for the 30% TiO
2−x NPs-embedded PDMS which became a positively charged material, leading to the drop of the TENG output performance, even though a strong applied pushing force. In addition, the trend of the TENG output among pristine, 5%, and 30% is the same as the measurement at 5 N and 5 Hz shown in
Figure 2. It was noted that the surrounding conditions were 75% relative humidity and 32 °C room temperature for the different applied forces measurements.
Figure 2c shows the effect of voltage and current characteristics of the TENG as a function of external load resistance ranging from 0.1 to 1000 MΩ. These measurements were performed under a pushing force and frequency of 5 N and 5 Hz, respectively. As shown in
Figure 2c, the TENG voltage increased by increasing the resistance from 0.1 to 200 MΩ, while the current value followed the opposite trend. Afterward, both the voltage and current became saturated at very high load resistances (i.e., 200–1000 MΩ), and the TENG exhibited the highest voltage and lowest current values ranging from 230.6–260 V and 4.8–2.6 µA. In addition, the average power density (
Pavg) was calculated by the following the equation:
where
V and
I are the output peak voltage and current values of the TENG at various load resistances, respectively, and
S is the active area (i.e., 9 cm
2) of the TENG.
Figure 2d shows the effect of the TENG output power density as a function of external load resistance. Following
Figure 2d, the
Pavg values of TENG increased by increasing the load resistance and then decreased at a relatively high load resistance. Specifically, at the moderate load resistance of 40 MΩ, the TENG exhibited a maximum power density of 1.84 W.m
−2, under the pushing force and frequency of 5 N and 5 Hz, respectively. More discussion is provided below regarding the output performance behavior of the TENGs and the PDMS properties according to the TiO
2−x NP embedding ratio.
Previous studies show that as the embedded weight ratio of NPs with high dielectric constants increases, the TENG output performance was improved because of the increasing dielectric constant of the tribo-material [
13]. Our results show the same trends as previous studies, as shown in
Figure 3a. In addition, the dielectric constant according to frequency does not change significantly. However, we provide below not only an increase in the dielectric constant of the tribo-material but also suggest an additional mechanism based on the role of oxygen vacancy in TiO
2−x NP embedded PDMS to effectively enhance TENG performance. To investigate changes of chemical bonding state within the PDMS layer according to the amount of embedded TiO
2−x NPs, the oxygen (O) 1
s spectra of PDMS and TiO
2−x NPs 5% embedded PDMS layers were observed via XPS, as shown in
Figure 3b. For the detailed analysis of chemical bonding states, the O 1
s spectra were carefully normalized and de-convoluted with three different Gaussian peaks as indexed with O1, O2, and O3 centered at 530.9 eV, 531.8 eV, and 532.9 eV, respectively. Each of the representatively assigned peaks from a low binding energy is related to the oxygen state in the metal-oxide lattices, the oxygen-deficient state, and chemisorbed or dissociated oxygen states, or OH
− impurities, respectively [
14,
15]. Among them, the relative area of the oxygen-deficient peak (O2) is dramatically increased from 18.80% to 24.63% after TiO
2−x NPs embedding, which is remarkable. Moreover, we measured and de-convoluted O 1
s’ peak of other films that have different concentration, as shown in
Figure S3. In the result, the oxygen-deficient states were similar regardless of increases of TiO
2−x concentration. This saturation can be observed due to the formation of TiO
2−x clusters in the composite film (see
Figure 1d). The TiO
2−x nanoparticles in a cluster act like a single particle. This means that the number of active oxygen deficient states are as same as a single TiO
2−x nanoparticle. Due to the oxygen vacancies being electrically positively charged, the increment of oxygen vacancies of the negative tribo-material surface could induce electron flow from the top electrode by the attraction force, as shown in
Figure 3c. Therefore, the TiO
2−x NPs-embedded PDMS layer has a larger oxygen-deficient state by oxygen vacancies, which can contribute to an enhanced TENG performance. To theoretically understand the output performance enhancement of the TiO
2−x NPs-embedded TENG, a COMSOL Multiphysics (5.0, COMSOL, Inc.) simulation was conducted.
Figure 3d shows the corresponding results for the triboelectric potential distributions of pristine TENGs and TiO
2−x NPs-embedded TENG, respectively. The details of the COMSOL Multiphysics simulation parameters and equations are provided in our previous study, Reference [
16]. As a result, the COMSOL simulations showed that the 5% TiO
2−x NPs-embedded TENG can exhibit higher performance than the pristine TENG.
To elucidate the cause of the significantly decreased output performance of TENG containing over 5% embedding TiO
2−x NPs, the correlation between the electronic structures of the TiO
2−x NPs-embedded PDMS and the energy conversion mechanism of the TENG were investigated.
Figure 4a shows the hybridized molecular orbital structures in the conduction band of the TiO
2−x NPs-embedded PDMS as a function of the weight ratio of TiO
2−x NPs measured by XAS. The normalized intensities of the oxygen K-edge spectra of pristine PDMS and TiO
2−x NPs-embedded PDMS layers directly reflect the unoccupied hybridized states by the transition of electrons from the occupied O 1
s state [
17].
Figure 4a co-plots the normalized O-K edge XAS spectrum of TiO
2−x NPs (gray lines) for easy comparison with the changes in the TiO
2−x NPs-embedded PDMS layer spectra. In particular, XAS analysis is a surface sensitive analytical method that measures the current flowing on the sample surfaces after incident X-ray exposure. Therefore, this is suitable for analyzing tribo-materials whose output performance changes according to surface conditions. The XAS spectra of TiO
2−x NPs are located in the two strong resonance peaks at 531.5 and 534 eV [
18]. With an increased weight ratio of TiO
2−x NPs from 0 to 30%, the electronic structure of PDMS is clearly changed by the addition of the electronic structure of TiO
2−x NPs. These changes in the tribo-material surface can cause changes in the tribo-series, resulting in reduced tribo-electrification effects. For the experimental demonstration of our claim, KPFM measurements were carried out to detect the surface potential of different surfaces according to the weight ratio of TiO
2−x NPs, as shown in
Figure 4b. As the weight ratio of TiO
2−x NPs increased from 0 to 30%, the average surface potential dramatically changed. Specifically, the TiO
2−x NPs 30% sample became a positively charged material. Moreover, considering the SEM image in
Figure 1d, the electron path can be formed due to NPs clustering in the case of the TENG containing over 5% embedding TiO
2−x NPs. The electron path formed by the NPs cluster can move the electrons induced on the surface and increase the leakage current, as shown in
Figure S4 (supporting information), which may be a reasonable cause to reduce TENG performance above 5% embedding TiO
2−x NPs, as shown in
Figure 4c. To demonstrate this with a practical application, we designed a windmill system to harvest the wind energy utilizing the pristine TENG and optimal TENG devices (TiO
2−x NPs 5% embedded TENG), as shown in
Figure 5a. In the presence of wind flow, the windmill blades are forced to rotate and lead to the rotation of a quad nose cam. Subsequently, the quad nose cam transmits its rotation motion to linear motion on the top plate of the TENG. Resulting from that motion, the TENG operates in the vertical direction via contact and separation mode repeatedly (
Figure 5b), which produces the TENG electrical output. Moreover, the relation of wind speed and output performance of the windmill-integrated TENG was also analyzed at various wind speeds, as shown in
Figure 5c. The measured voltage is clearly shown in the output performance of both the pristine and optimal TENGs, which show linear enhancement upon increasing the wind speed applied to the windmill blades. The peak voltage values of the windmill attached to pristine TENG at the wind speeds of ~10, 15, 20, 25, 30, and 35 are 70, 92, 114, 130, 182, and 190, and that for the windmill integrated with an optimal TENG are 94, 172, 220, 268, 304, and 304, respectively. The output data in
Figure 5c also show a linear enhancement regarding the number of pushing cycles, i.e., pushing frequency and force on the top plate of the TENG as the wind speed increases. With faster wind speeds, the output performance of the windmill TENG can be enhanced. The results clearly demonstrate that our windmill TENG system can efficiently harvest wind energy.