Article

Production of (Fe,Co)Si2 and (Fe.Mn)Si2 Thermoelectric Materials by Spark Plasma Sintering

1
Department of Advanced Materials Science and Engineering, Chiba Institute of Technology, Narashino, Chiba 275-8588, Japan
2
Pacific Steel Mfg. Co., Ltd., Toyama 930-0808, Japan
*
Author to whom correspondence should be addressed.
Crystals 2024, 14(1), 56; https://doi.org/10.3390/cryst14010056
Submission received: 2 December 2023 / Revised: 28 December 2023 / Accepted: 29 December 2023 / Published: 30 December 2023

Abstract

:
In this study, FeSi2 bulk specimens were prepared by mechanical alloying, spark plasma sintering, and subsequent annealing. The annealed FeSi2 bulk specimens consisted of the β-FeSi2 phase and exhibited high Seebeck coefficient values. The maximum Seebeck coefficient of 356 μVK−1 was achieved in the FeSi2 bulk specimen annealed at 1173 K for 6 h. However, the power factor of the FeSi2 bulk specimen was quite small due to its high electrical resistivity, and a drastic improvement is required. Therefore, Mn- and Co-substituted specimens, Fe1−xMnxSi2 (x = 0.2–0.8) and Fe1−xCoxSi2 (x = 0.2–0.8), were produced, and their thermoelectric properties were evaluated. The Mn- and Co-substituted specimens exhibited lower electrical resistivity and a higher power factor than the FeSi2 bulk specimen. The Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens were p-type thermoelectric materials, and a Seebeck coefficient of 262 μVK−1 and a power factor of 339 μWm−1K−2 were achieved in the Fe0.94Mn0.06Si2 bulk specimen. On the other hand, the Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens were n-type thermoelectric materials, and a Seebeck coefficient of −180 μVK−1 and a power factor of 667 μWm−1K−2 were achieved in the Fe0.96Co0.04Si2 bulk specimen.

1. Introduction

Humanity is facing the critical issue of preventing or at least slowing the progress of global warming, which is known to be caused by greenhouse gases, particularly those emitted by burning fossil fuels such as coal and oil. Although burning such fossil fuels is still necessary to secure energy supplies, more than 60% of the energy generated is lost as waste heat [1]. Thus, research on waste heat recovery is currently a focus of attention [2,3,4]. Various studies on technologies for waste heat recovery have been reported [5,6]. One of the techniques to recover waste heat is thermoelectric generation, which can convert waste heat to electricity by means of thermoelectric materials.
Until now, only the bismuth telluride (Bi2Te3) compound has been used in thermoelectric modules such as those for the electric cooling of computer devices [7,8,9,10,11,12]. However, Bi2Te3 cannot be used for thermoelectric generation because it consists of scarce and toxic elements. The iron silicide (β-FeSi2) compound, another thermoelectric material, consists of nontoxic and abundant elements. The thermoelectric properties of the β-FeSi2 compound have been studied, and numerous efforts have been made to produce it [13,14,15,16,17,18,19]. Unfortunately, the β-FeSi2 compound is found to be a peritectoid phase, which is difficult to produce from the melt. It exhibits an unfavorably high electric resistance for a thermoelectric material.
From the viewpoint of achieving the Sustainable Development Goals (SDGs) formulated by the United Nations, the use of nontoxic β-FeSi2 compound as a thermoelectric material to realize thermoelectric generation for waste heat recovery is attracting renewed interest. It has been found that sintering is a suitable method for obtaining the β-FeSi2 compound [20,21] and that the thermoelectric properties of the β-FeSi2 compound are improved by the addition of Co or Mn [22,23]. However, the amount of the Co or Mn added to the β-FeSi2 compound needs to be optimized to improve its thermoelectric properties [24]. Therefore, further studies are necessary to improve these compounds.
The thermoelectric properties of the β-FeSi2 compounds are deeply dependent on the processing conditions. β-FeSi2 compounds have been produced by sintering of elemental powder mixtures or Fe-Si alloy powder with the composition of FeSi2 [18,25], but it was found that β-FeSi2 compounds produced by mechanical alloying and subsequent spark plasma sintering exhibited better thermoelectric properties [19,26]. Therefore, we produced β-FeSi2 compounds and those Co-doped and Mn-doped specimens by mechanical alloying and spark plasma sintering. The thermoelectric properties of the resultant β-FeSi2 compounds were systematically investigated.

2. Materials and Methods

2.1. Mechanical Alloying (MA)

Elemental Fe (99.9%) and Si (99.9%) were weighed and then mixed with a mortar and pestle in an argon-filled glove box (argon purity: 99.99%). The nominal composition of the powder mixture was Fe-66.7at%Si (FeSi2). The mixed powder of 40 g in weight was poured into a cylindrical steel container together with steel balls (10 mm in diameter) having a total weight of 400 g and then sealed in an argon-filled glove box. Mechanical alloying of the mixed powders was performed for 20 h with a ball-to-powder ration of 10:1 using a planetary ball mill at a rotation speed of 250 rpm (FRITSCH: Planetary Mono Mill PULVERRISETTE 6, Idar-Oberstein, Germany). The planetary ball mill is known as a high-energy ball mill. Details of the planetary ball mill are described elsewhere [27]. After the mechanical alloying, the powder was removed from the container in the argon-filled glove box. The same procedure was used to prepare powder mixtures of Fe1−xMnxSi2 (x = 0.2–0.8) and Fe1−xCoxSi2 (x = 0.2–0.8).

2.2. Spark Plasma Sintering

Samples of the mechanically alloyed FeSi2 powder of 1 g in weight were put into a carbon die and consolidated into bulk materials by the spark plasma sintering method. The consolidation was performed in a vacuum at 1073 K for 300 s under a pressure of 100 MPa. Bulk specimens were prepared under vacuum by the SPS method using a spark plasma sintering apparatus (Plasman, S. S. Alloy, Hiroshima, Japan). The temperature of the specimen was increased from room temperature to the consolidating temperature of 973 K over a period of 300 s and then held at the consolidating temperature for 300 s, in accordance with the SPS method. After the specimens were cooled to room temperature, they were taken from the carbon die and subsequently annealed at 1073–1173 K for 6–20 h in an argon atmosphere. The bulk materials of Fe1−xMnxSi2 (x = 0.2–0.8) and Fe1−xCoxSi2 (x = 0.2–0.8) were annealed at 1173 K for 6 h in an argon atmosphere.

2.3. Characterization

The mechanically alloyed powders and bulk materials were characterized by X-ray diffraction (XRD) using Cu Kα radiation (MiniFlex600, Rigaku, Tokyo, Japan), and the morphology of the specimens was investigated using a scanning electron microscope (JSM-IT300LA, JEOL, Tokyo, Japan). The thermal properties of the specimens were measured in an argon atmosphere at a heating rate of 0.16 K/s using a differential thermal analysis (STA7300, Hitachi-hightech, Tokyo, Japan). Samples measuring 1 × 1 × 8 mm were cut out from the bulk materials using a low-speed diamond saw, and the Seebeck coefficient and electrical resistivity of the specimens were measured by the standard DC four-probe technique in a helium atmosphere using a ZEM-3 Seebeck Coefficient/Electric Resistance Measurement System (Advance Riko, Inc., Kanagawa, Japan). The power factor of the specimens was obtained from the Seebeck coefficient and electrical resistivity values.

3. Results and Discussion

3.1. FeSi2 Compound

The mechanically alloyed FeSi2 powder was consolidated at 1073 K into a bulk specimen. Figure 1 shows the XRD patterns of the mechanically alloyed powder, the bulk specimen, and the annealed bulk specimen. The binary phase diagram of the Fe-Si system alloys is shown in Figure 2 [28]. The XRD pattern of the mechanically alloyed powder prepared from the powder mixture with the nominal composition of FeSi2 showed diffraction peaks of the α-Fe phase together with small and broad diffraction peaks of the Si phase. There have been several reports on the formation of the β-FeSi2 phase by mechanical alloying [29,30], but the mechanically alloyed powder in the present study did not contain the β-FeSi2 phase. On the other hand, diffraction peaks of ε-FeSi and α-Fe2Si5 phases were found in the XRD pattern of the bulk specimen consolidated at 1073 K. According to the Fe-Si phase diagram, the equilibrium phase in this specimen is the β-FeSi2 phase at 1073 K. However, the bulk specimen consisted of ε-FeSi and α-Fe2Si5 phases. The β-FeSi2 phase is a peritectoid phase that is formed by a peritectoid reaction from ε-FeSi and α-Fe2Si5 phases. Thus, a bulk specimen consisting of the β-FeSi2 phase could be obtained by annealing the bulk specimen containing ε-FeSi and α-Fe2Si5 phases. The XRD pattern of the bulk specimen annealed at 1073 K for 6 h exhibited diffraction peaks of the β-FeSi2 phase, indicating that annealing is necessary to obtain the β-FeSi2 phase. These results suggest that mechanical alloying, spark plasma sintering, and subsequent annealing can produce the specimens consisting of the β-FeSi2 phase.
In order to confirm the existence of the β-FeSi2 phase in the FeSi2 bulk specimen annealed at 1073 K for 6 h, the thermal properties of the FeSi2 bulk specimen were examined by DTA. Figure 3 shows the DTA curve of the FeSi2 bulk specimen annealed at 1073 K for 6 h. The curve shows one large endothermic peak at around 1260 K, corresponding to the peritectoid reaction temperature (β-FeSi2 phase → ε-FeSi and α-Fe2Si5 phases). This suggests that the FeSi2 bulk specimen annealed at 1073 K for 6 h consisted of the β-FeSi2 phase.
The thermoelectric properties of the FeSi2 bulk specimens annealed at 1073 K, 1123 K, and 1173 K for 6 h were examined. The Seebeck coefficient and electrical resistivity of the specimens are shown in Figure 4 and Figure 5, respectively. The bulk specimen without annealing is also shown for comparison. These specimens are found to be p-type thermoelectric materials, which are characterized by a positive Seebeck coefficient. The Seebeck coefficient of the bulk specimen without annealing was very small, whereas that of the annealed specimens was quite large. This confirms that the annealed specimens consisting of the β-FeSi2 phase exhibited a large Seebeck coefficient. Regardless of the ambient temperature, the bulk specimens annealed at higher annealing temperatures showed a higher Seebeck coefficient. The maximum Seebeck coefficient of 356 μVK−1 was achieved in the bulk specimen annealed at 1173 K for 6 h. This value is comparable or superior to that of the Bi2Te3 compound. The annealed bulk specimens can thus be considered to be promising candidates for thermoelectric materials. A further increase in the annealing temperature may increase the Seebeck coefficient value, but it should be noted that the annealing was performed at temperatures lower than that of the eutectoid reaction (Fe2Si3 → β-FeSi2 + Si), which takes place at 1210 K.
The bulk specimen without annealing had a low electrical resistivity of 64 μΩm at room temperature. On the other hand, the annealed bulk specimens consisting of the β-FeSi2 phase exhibited high electrical resistivity at room temperature, ranging from 17,600 μΩm for the specimen annealed at 1073 K to 8000 μΩm for the specimen annealed at 1173 K. Furthermore, the electrical resistivity of the annealed bulk specimens drastically decreased as the ambient temperature increased, indicating that the annealed bulk specimens exhibit semiconductor-like temperature dependency. This confirms that the annealed bulk specimens consisted of the semiconducting β-FeSi2 phase.
The power factors of the FeSi2 bulk specimen and those annealed at 1073 K, 1123 K, and 1173 K for 6 h were calculated using equation PF = S2/ρ, where PF is the power factor, S is the Seebeck coefficient and ρ is electrical resistivity. The results are shown in Figure 6. Unfortunately, the power factors of the annealed bulk specimen were less than 50 μWm−1K−2, two orders smaller than that of the Bi2Te3 compound (around 3000 μWm−1K−2). This is due to the high electrical resistivity of the annealed bulk specimens. Further studies are therefore necessary to reduce the electrical resistivity of the bulk specimens consisting of the β-FeSi2 phase.

3.2. (Fe,Mn)Si2 and (Fe,Co)Si2 Compound

In the initial part of the study described above, a β-FeSi2 specimen with a high Seebeck coefficient was obtained by annealing the bulk specimens at 1173 K for 6 h. Thus, Fe1−xMnxSi2 (x = 0.2–0.8) and Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens were prepared using the same procedure. The (Fe,Mn)Si2 and (Fe,Co)Si2 phases were successfully obtained through this process.
First, the thermoelectric properties of Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens annealed at 1173 K for 6 h were compared with those of the FeSi2 bulk specimen annealed at 1173 K for 6 h. The Seebeck coefficient and electrical resistivity of the specimens are shown in Figure 7 and Figure 8, respectively. The Seebeck coefficient of the annealed FeSi2 bulk specimen was higher than that of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens in the ambient temperature range used in this experiment. The annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens were found to be p-type thermoelectric materials, as was the case for the annealed FeSi2 bulk specimen. At room temperature, the Seebeck coefficient of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens increased from 38.6 μVK−1 for Fe0.98Mn0.02Si2 to 262 μVK−1 for Fe0.94Mn0.06Si2 and then decreased, as the Mn content further increased, to 27.3 μVK−1 for Fe0.92Mn0.08Si2.
The electrical resistivity of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens was also lower than that of the annealed FeSi2 bulk specimen in the ambient temperature range used in this experiment. At room temperature, the electrical resistivity of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens slightly increased from 303 μΩm for Fe0.98Mn0.02Si2 to 1060 μΩm for Fe0.94Mn0.06Si2 and then decreased, as the Mn content further increased, to 134 μΩm for Fe0.92Mn0.08Si2. This suggests that Mn substitution effectively reduces the electrical resistivity of the annealed FeSi2 bulk specimen. The electrical resistivity of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens exhibited a semiconductor-like temperature dependency, as was the case for the annealed FeSi2 bulk specimen.
The power factor of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens was calculated, and the results are shown in Figure 9. It was found that the power factor of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens also increased as the ambient temperature increased. Regardless of the ambient temperature, the annealed Fe0.94Mn0.06Si2 bulk specimen showed a higher power factor than the other annealed bulk specimens. The maximum power factor of 339 μWm−1K−2 was achieved in the annealed Fe0.94Mn0.06Si2 bulk specimen measured at 600 K. This value is much higher than that of the annealed FeSi2 bulk specimen but still smaller than that of the Bi2Te3 compound.
Secondly, the thermoelectric properties of Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens annealed at 1173 K for 6 h were compared with those of the FeSi2 bulk specimen annealed at 1173 K for 6 h. The Seebeck coefficient and electrical resistivity of the specimens are shown in Figure 10 and Figure 11, respectively. Unlike the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens, the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens exhibited a negative Seebeck coefficient. The annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens were found to be n-type thermoelectric material. The absolute values of the Seebeck coefficients of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens were lower than that of the annealed FeSi2 bulk specimen. At room temperature, the absolute values of the Seebeck coefficients of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens increased from −64.7 μVK−1 for Fe0.98Co0.02Si2 to −180 μVK−1 for Fe0.96Co0.04Si2 and then decreased as the Co content further increased, to −35.2 μVK−1 for Fe0.92Co0.08Si2.
The electrical resistivity of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens was lower than that of the annealed FeSi2 bulk specimen, as was the case for the Mn substitution. At room temperature, the electrical resistivity of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens slightly increased from 64.6 μΩm for Fe0.98Co0.02Si2 to 108 μΩm for Fe0.96Co0.04Si2 and then decreased, as the Co content further increased, to 13.8 μΩm for Fe0.92Co0.08Si2. This suggests that Co substitution is also effective in reducing the electrical resistivity of the annealed FeSi2 bulk specimen. The electrical resistivity of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens also exhibit semiconductor-like temperature dependency, as was the case for the annealed FeSi2 bulk specimen.
The power factor of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimens was calculated, and the results are shown in Figure 12. It was found that the power factor of the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimen also increased as the ambient temperature increased. The annealed Fe0.96Co0.04Si2 bulk specimen showed a higher power factor than the other bulk specimens. The maximum power factor of 667 μWm−1K−2 was achieved in the annealed Fe0.96Co0.04Si2 bulk specimen measured at 600 K. This value is higher than that of the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens.
The Seebeck coefficient of the Mn- and Co-substituted FeSi2 specimens is almost comparable to the commercial Bi-Te thermoelectric compound (180–200 μVK−1). However, the power factor of the Mn- and Co-substituted FeSi2 specimens is inferior to that of the Bi-Te thermoelectric compound (2000–3000 μWm−1K−2). Thus, further improvement of the power factor is essential in order to realize thermoelectric materials for thermoelectric generation to achieve waste heat recovery.

4. Conclusions

The FeSi2 bulk specimens prepared by spark plasma sintering from the mechanically alloyed powder consisted of FeSi and Fe2Si3 phases and showed a low Seebeck coefficient. The annealed FeSi2 bulk specimens consisted of the β-FeSi2 phase and exhibited a high Seebeck coefficient, reaching a maximum of 356 μVK−1 for the FeSi2 bulk specimens annealed at 1173 K for 6 h. However, the power factor of the annealed FeSi2 bulk specimen was less than 50 μWm−1K−2 due to the high electrical resistivity. Thus, Mn- and Co-substituted specimens were prepared using the same procedure to improve the power factor. Although the Mn and Co substitutions decreased the Seebeck coefficient, the substitutions significantly reduced the electrical resistivity and increased the power factor. It was also found that the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens were p-type thermoelectric materials, whereas the annealed Fe0.96Co0.04Si2 bulk specimens were n-type thermoelectric materials. Among the annealed Fe1−xMnxSi2 (x = 0.2–0.8) bulk specimens, the Fe0.94Mn0.06Si2 bulk specimen exhibited a Seebeck coefficient of 262 μVK−1 and a power factor of 339 μWm−1K−2. Among the annealed Fe1−xCoxSi2 (x = 0.2–0.8) bulk specimen, on the other hand, the Fe0.96Co0.04Si2 bulk specimen showed a Seebeck coefficient of −180 μVK−1 and a power factor of 667 μWm−1K−2.

Author Contributions

T.S.: Methodology, Writing, Formal analysis, Original Draft preparation; R.A.: Methodology, Investigation, Formal analysis. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by a Grant-in-Aid from the Amada Foundation (AF-2021016-B3).

Data Availability Statement

Data are contained within the article.

Acknowledgments

We are grateful for a Grant-in-Aid from the Amada Foundation.

Conflicts of Interest

Author Ryoki Asakawa was employed by the company Pacific Steel Mfg. Co., Ltd. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Zhang, X.; Zhao, L.D. Thermoelectric materials: Energy conversion between heat and electricity. J. Mater. 2015, 1, 92–105. [Google Scholar] [CrossRef]
  2. Jouhara, H.; Olabi, A.G. Editorial: Industrial waste heat recovery. Energy 2018, 160, 1–2. [Google Scholar] [CrossRef]
  3. Brückner, S.; Liu, S.; Miró, L.; Radspieler, M.; Cabeza, L.F.; Lävemann, E. ndustrial waste heat recovery technologies: An economic analysis of heat transformation technologies. Appl. Energy 2015, 151, 157–167. [Google Scholar] [CrossRef]
  4. Law, R.; Harvey, A.; Reay, D. A knowledge-based system for low-grade waste heat recovery in the process industries. Appl. Therm. Eng. 2016, 94, 590–599. [Google Scholar] [CrossRef]
  5. Huang, F.; Zheng, J.; Baleynaud, J.M.; Lu, J. Heat recovery potentials and technologies in industrial zones. J. Energy Inst. 2017, 90, 951–961. [Google Scholar] [CrossRef]
  6. Jouhara, H.; Khordehgah, N.; Almahmoud, S.; Delpech, B.; Chauhan, A.; Tassou, S.A. Waste Heat Recovery Technologies and Applications. Therm. Sci. Eng. Prog. 2018, 6, 268–289. [Google Scholar] [CrossRef]
  7. Satterthwaite, C.B.; Ure, R.W., Jr. Electrical and Thermal Properties of Bi2Te3. Phys. Rev. 1957, 108, 1164–1170. [Google Scholar] [CrossRef]
  8. Rosi, F.D.; Abeles, B.; Jensen, R.V. Materials for thermoelectric refrigeration. J. Phys. Chem. Solids 1959, 10, 191–200. [Google Scholar] [CrossRef]
  9. Wada, H.; Sato, T.; Takahashi, K.; Nakatsukasa, K. The anisotropic powder metallurgy of n-type Bi2Te2.85Se0.15 thermoelectric material. J. Mater. Res. 1990, 5, 1052–1057. [Google Scholar] [CrossRef]
  10. Goldsmid, H.J. Bismuth Telluride and Its Alloys as Materials for Thermoelectric Generation. Materials 2014, 7, 2577–2592. [Google Scholar] [CrossRef]
  11. Mamur, H.; Bhuiyan, M.R.A.; Korkmaz, F.; Nil, M. A review on bismuth telluride (Bi2Te3) nanostructure for thermoelectric applications. Renew. Sust. Energ. Rev. 2018, 82, 4159–4169. [Google Scholar] [CrossRef]
  12. Thakur, V.; Upadhyay, K.; Kaur, R.; Goyal, N.; Gautam, S. Investigating phase transition and morphology of Bi-Te thermoelectric system. Mater. Today Adv. 2020, 8, 100082. [Google Scholar] [CrossRef]
  13. Ware, M.; McNeill, D.J. Iron disilicide as a thermoelectric generator materials. Proc. Inst. Electr. Eng. 1964, 111, 178–182. [Google Scholar] [CrossRef]
  14. Birkholz, U.; Schelm, J. Electrical Investigation of the Semiconductor-to-Metal Transition in FeSi2. Phys. Stat. Sol. B 1969, 34, K177–K180. [Google Scholar] [CrossRef]
  15. Nishida, I. Study of Semiconductor-to-Metal Transition in Mn-Doped FeSi2. Phys. Rev. B 1973, 7, 2710–2713. [Google Scholar] [CrossRef]
  16. Piton, J.P.; Fay, M.F. Phase changes in iron–silicon alloys around the composition FeSi2. Acad. C. R. Sci. 1968, C266, 514–516. [Google Scholar]
  17. Kojima, T. Semiconducting and Thermoelectric Properties of Sintered Iron Disilicide. Phys. Stat. Sol. A 1989, 111, 233–242. [Google Scholar] [CrossRef]
  18. Dąbrowski, F.; Ciupiński, Ł.; Zdunek, J.; Kruszewski, J.; Zybała, R.; Michalski, A.; Kurzydłowski, K.J. Microstructure and thermoelectric properties of p and n type doped β-FeSi2 fabricated by mechanical alloying and pulse plasma sintering. Mater. Today Proc. 2019, 8, 531–539. [Google Scholar] [CrossRef]
  19. Ohta, Y.; Miura, S.; Mishima, Y. Thermoelectric semiconductor iron disilicides produced by sintering elemental powders. Intermetallics 1999, 7, 1203–1210. [Google Scholar] [CrossRef]
  20. Qu, X.; Lü, S.; Hu, J.; Meng, Q. Microstructure and thermoelectric properties of β-FeSi2 ceramics fabricated by hot-pressing and spark plasma sintering. J. Alloys Compd. 2011, 509, 10217–10221. [Google Scholar] [CrossRef]
  21. Nogi, K.; Kita, T. Rapid production of β-FeSi2 by spark-plasma sintering. J. Mater. Sci. 2000, 35, 5845–5849. [Google Scholar] [CrossRef]
  22. Ito, M.; Nagai, H.; Tanaka, T.; Katsuyama, S.; Majima, K. Thermoelectric performance of n-type and p-type β-FeSi2 prepared by pressureless sintering with Cu addition. J. Alloys Compd. 2001, 319, 303–311. [Google Scholar] [CrossRef]
  23. Kim, S.W.; Cho, M.K.; Mishima, Y.; Choi, D.C. High temperature thermoelectric properties of p- and n-type β-FeSi2 with some dopants. Intermetallics 2003, 11, 399–405. [Google Scholar] [CrossRef]
  24. Pandey, T.; Singh, D.J.; Parker, D.; Singh, A.K. Thermoelectric properties of β-FeSi2. J. Appl. Phys. 2013, 114, 153704. [Google Scholar] [CrossRef]
  25. Abbassi, L.; Mesguich, D.; Coulomb, L.; Chevallier, G.; Aries, R.; Estournès, C.; Flahaut, E.; Viennois, R.; Beaudhuina, M. In-situ reactive synthesis of dense nanostructured β-FeSi2 by Spark Plasma Sintering. J. Alloys Compd. 2022, 902, 163683. [Google Scholar] [CrossRef]
  26. Yamada, H.; Katsumata, H.; Yuasa, D.; Uekusa, S.; Ishiyama, M.; Souma, H.; Azumaya, I. Structural and electrical properties of β-FeSi2 bulk materials for thermoelectric applications. Phys. Procedia 2012, 23, 13–16. [Google Scholar] [CrossRef]
  27. Broseghini, M.; Gelisioa, L.; D’Incaua, M.; Azanza Ricardoa, C.L.; Pugno, N.M.; Scardi, P. Modeling of the planetary ball-milling process: The case study of ceramic powders. J. Eur. Cerm. Soc. 2016, 9, 2205–2212. [Google Scholar] [CrossRef]
  28. Kubaschewski, O. Iron-Binary Phase Diagram; Springer: New York, NY, USA, 1982; pp. 136–137. [Google Scholar]
  29. Le Caër, G.; Bauer-Grosse, E.; Pianelli, A.; Bouzy, E.; Matteazzi, P. Mechanically driven syntheses of carbides and silicides. J. Mater. Sci. 1990, 25, 4726–4731. [Google Scholar] [CrossRef]
  30. Umemoto, M. Preparation of Thermoelectric β-FeSi2 Doped with Al and Mn by Mechanical Alloying (Overview). Mater. Trans. JIM 1995, 36, 373–383. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of (a) the mechanically alloyed FeSi2 powder, (b) the bulk specimen, and (c) the bulk specimen annealed at 1073 K for 6 h.
Figure 1. XRD patterns of (a) the mechanically alloyed FeSi2 powder, (b) the bulk specimen, and (c) the bulk specimen annealed at 1073 K for 6 h.
Crystals 14 00056 g001
Figure 2. Binary Phase diagram of Fe-Si system alloys [30].
Figure 2. Binary Phase diagram of Fe-Si system alloys [30].
Crystals 14 00056 g002
Figure 3. DTA curve of the FeSi2 bulk specimen annealed at 1073 K for 6 h.
Figure 3. DTA curve of the FeSi2 bulk specimen annealed at 1073 K for 6 h.
Crystals 14 00056 g003
Figure 4. Seebeck coefficient as a function of ambient temperature for (a) the FeSi2 bulk specimen without annealing and those annealed at (b) 1073 K, (c) 1123 K, and (d) 1173 K.
Figure 4. Seebeck coefficient as a function of ambient temperature for (a) the FeSi2 bulk specimen without annealing and those annealed at (b) 1073 K, (c) 1123 K, and (d) 1173 K.
Crystals 14 00056 g004
Figure 5. Electrical resistivity as a function of ambient temperature for (a) the FeSi2 bulk specimen without annealing and those annealed at (b) 1073 K, (c) 1123 K, and (d) 1173 K.
Figure 5. Electrical resistivity as a function of ambient temperature for (a) the FeSi2 bulk specimen without annealing and those annealed at (b) 1073 K, (c) 1123 K, and (d) 1173 K.
Crystals 14 00056 g005
Figure 6. Power factor as a function of ambient temperature for (a) the FeSi2 bulk specimen without annealing and those annealed at (b) 1073 K, (c) 1123 K, and (d) 1173 K.
Figure 6. Power factor as a function of ambient temperature for (a) the FeSi2 bulk specimen without annealing and those annealed at (b) 1073 K, (c) 1123 K, and (d) 1173 K.
Crystals 14 00056 g006
Figure 7. Seebeck coefficient as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Mn0.02Si2, (c) Fe0.96Mn0.04Si2, (d) Fe0.94Mn0.06Si2, and (e) Fe092Mn0.08Si2 bulk specimens.
Figure 7. Seebeck coefficient as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Mn0.02Si2, (c) Fe0.96Mn0.04Si2, (d) Fe0.94Mn0.06Si2, and (e) Fe092Mn0.08Si2 bulk specimens.
Crystals 14 00056 g007
Figure 8. Electrical resistivity as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Mn0.02Si2, (c) Fe0.96Mn0.04Si2, (d) Fe0.94Mn0.06Si2, and (e) Fe092Mn0.08Si2 bulk specimens.
Figure 8. Electrical resistivity as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Mn0.02Si2, (c) Fe0.96Mn0.04Si2, (d) Fe0.94Mn0.06Si2, and (e) Fe092Mn0.08Si2 bulk specimens.
Crystals 14 00056 g008
Figure 9. Power factor as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Mn0.02Si2, (c) Fe0.96Mn0.04Si2, (d) Fe0.94Mn0.06Si2, and (e) Fe092Mn0.08Si2 bulk specimens.
Figure 9. Power factor as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Mn0.02Si2, (c) Fe0.96Mn0.04Si2, (d) Fe0.94Mn0.06Si2, and (e) Fe092Mn0.08Si2 bulk specimens.
Crystals 14 00056 g009
Figure 10. Seebeck coefficient as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Co0.02Si2, (c) Fe0.96Co0.04Si2, (d) Fe0.94Co0.06Si2, and (e) Fe092Co0.08Si2 bulk specimens.
Figure 10. Seebeck coefficient as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Co0.02Si2, (c) Fe0.96Co0.04Si2, (d) Fe0.94Co0.06Si2, and (e) Fe092Co0.08Si2 bulk specimens.
Crystals 14 00056 g010
Figure 11. Electrical resistivity as a function of ambient temperature for the (a) FeSi2 (dashed-line), (b) Fe0.98Co0.02Si2, (c) Fe0.96Co0.04Si2, (d) Fe0.94Co0.06Si2, and (e) Fe092Co0.08Si2 bulk specimens.
Figure 11. Electrical resistivity as a function of ambient temperature for the (a) FeSi2 (dashed-line), (b) Fe0.98Co0.02Si2, (c) Fe0.96Co0.04Si2, (d) Fe0.94Co0.06Si2, and (e) Fe092Co0.08Si2 bulk specimens.
Crystals 14 00056 g011
Figure 12. Power factor as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Co0.02Si2, (c) Fe0.96Co0.04Si2, (d) Fe0.94Co0.06Si2, and (e) Fe092Co0.08Si2 bulk specimens.
Figure 12. Power factor as a function of ambient temperature for the (a) FeSi2 (dashed line), (b) Fe0.98Co0.02Si2, (c) Fe0.96Co0.04Si2, (d) Fe0.94Co0.06Si2, and (e) Fe092Co0.08Si2 bulk specimens.
Crystals 14 00056 g012
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Saito, T.; Asakawa, R. Production of (Fe,Co)Si2 and (Fe.Mn)Si2 Thermoelectric Materials by Spark Plasma Sintering. Crystals 2024, 14, 56. https://doi.org/10.3390/cryst14010056

AMA Style

Saito T, Asakawa R. Production of (Fe,Co)Si2 and (Fe.Mn)Si2 Thermoelectric Materials by Spark Plasma Sintering. Crystals. 2024; 14(1):56. https://doi.org/10.3390/cryst14010056

Chicago/Turabian Style

Saito, Tetsuji, and Ryoki Asakawa. 2024. "Production of (Fe,Co)Si2 and (Fe.Mn)Si2 Thermoelectric Materials by Spark Plasma Sintering" Crystals 14, no. 1: 56. https://doi.org/10.3390/cryst14010056

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.