Next Article in Journal
Orebody Modeling Method Based on the Coons Surface Interpolation
Next Article in Special Issue
Understanding the Entrainment Behavior of Gangue Minerals in Flake Graphite Flotation
Previous Article in Journal
Constraints on the Genesis of the Shuangwang Gold Deposit in Qinling Orogen, Central China: Evidence from In Situ Trace Element and Sulfur Isotope
Previous Article in Special Issue
Sodium N-Lauroylsarcosinate (SNLS) as a Selective Collector for Calcareous Phosphate Beneficiation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effect of Calcium Ion on the Flotation of Fluorite and Calcite Using Sodium Oleate as Collector and Tannic Acid as Depressant

1
School of Resources and Environmental Engineering, Wuhan University of Technology, Wuhan 430070, China
2
Hubei Key Laboratory of Mineral Resources Processing and Environment, Wuhan 430070, China
3
Zhejiang CPS Cathay Packing & Sealing Co., Ltd., Hangzhou 311255, China
4
Jiangxi Copper Technology Research Institute, Jiangxi Copper Corporation, Nanchang 330096, China
*
Author to whom correspondence should be addressed.
Minerals 2022, 12(8), 996; https://doi.org/10.3390/min12080996
Submission received: 13 July 2022 / Revised: 3 August 2022 / Accepted: 3 August 2022 / Published: 6 August 2022
(This article belongs to the Special Issue Advances in Non-metallic Ore Separation)

Abstract

:
In the flotation of semi-soluble minerals such as calcite and fluorite, Ca2+ is one of the common dissolved components influencing the collector adsorption behaviors on the mineral surfaces. However, there is very limited research focusing on how the dissolved Ca2+ affects the separation of fluorite and calcite. In the study, with sodium oleate (NaOL) as a collector and tannic acid (TA) as a depressant, a flotation test, zeta potential measurement, and adsorption experiment in the presence of Ca2+ were conducted. Flotation tests indicated that in the presence of Ca2+, fluorite and calcite were both significantly depressed by TA, leading to difficulty in the separation of the two minerals. It was also found that the depression effect on fluorite flotation was minimized with a high concentration of NaOL. Zeta potential measurement and the adsorption experiment results are consistent with the flotation results, revealing that it is only in the low concentration of NaOL that the flotation of fluorite was depressed by TA in the presence of Ca2+. Specifically, in the low concentration of NaOL, TA adsorbed on the fluorite surface and depressed the flotation of fluorite due to the preferential interaction between NaOL and Ca2+ in the solution leading to a shortage in the effective NaOL in the solution. In the high concentration of NaOL, the adsorbed TA on the fluorite surface was displaced by the excessive NaOL in the solution; hence, the flotation of fluorite was recovered. In contrast, TA always hinders the interaction of NaOL with calcite regardless of the presence and absence of Ca2+ and NaOL, hence, depressing the flotation of calcite. The study presented that a high concentration of NaOL may mitigate the negative effect of Ca2+ on the fluorite surface and improve the separation of fluorite from calcite.

1. Introduction

Fluorite (CaF2) is an important strategic mineral that is used primarily for the production of hydrofluoric acid and as a flux agent in steel making [1]. In practice, calcite is one of the common gangue minerals in fluorite ore [2]. Froth flotation has been considered one of the most effective ways to separate fluorite from calcite. Fatty acids and their salts, such as sodium oleate (NaOL), were usually realized as collectors for fluorite and calcite flotation [3,4,5]. A comprehensive review of the interaction of NaOL onto the fluorite and calcite was reported as chemisorption, followed by the formation of hydrophobic aggregates and surface precipitation of calcium carboxylate from bulk solution [6,7,8]. In addition, the interaction of NaOL on fluorite and calcite surface is recognized mainly through chemisorption and physical adsorption, respectively [9]. Due to the similar surface properties and chemical reactivity with reagents [10], the separation of fluorite and calcite is relatively difficult, and a selectively depressant is considered the key to their separation.
Many calcite depressants were identified by researchers for the separation of fluorite and calcite, including inorganic and organic [11]. Due to the limit, pH application range, and the dewatering problem of the inorganic depressants, the organic depressants, such as tannic acid [1], psyllium seed gum [12], and sulfonated lignite [13], can selectively adsorb with Ca2+ on the calcite surface, have become an important direction in studying the separation of fluorite and calcite. Tannic Acid (TA) is one of the most widely used organic reagents for the depression of calcareous and siliceous ores in industry. In the case of calcite flotation, Castro et al. [11] demonstrated that the effect of quebracho, a tannic acid extract is more effective on calcite than on celestite. Yuehua Hu et al. [1] identified the selective adsorption of TA on calcite via Ca2+ and Ca(OH)+ components on the mineral surface and depressed calcite in the fluorite flotation using NaOL as a collector. However, the results of a bench-scale flotation test for a fluorite ore flotation from Hunan, Chenzhou, were not good enough without hydrochloric acid adjustment using NaOL as collector and TA as depressant [14]. Considering the species, especially calcium ion dissolved from calcium-bearing minerals, is inevitable during a long flotation processing, the floatability of fluorite and calcite may be different in a high Ca2+ content flotation slurry [15,16,17].
It is documented that the interaction between the collector and Ca2+ in bulk solution dominated the collector adsorption mechanism at these mineral surfaces [18]. For example, Yijun Cao et al. [15] noted that both scheelite and fluorite were depressed strongly by sodium silicate in the presence of calcium. Many researchers also indicated that the Ca2+ adsorbed on mineral surface or suspended in solution would also consume the flotation reagent by precipitating into calcium salts, which would significantly reduce the flotation recovery of scheelite [8,19,20]. These investigations provided valuable information for the current study. However, in the fluorite and calcite flotation system, the adsorption mechanisms of NaOL and TA on the mineral surface in the presence of Ca2+ have not been reported. It was still hard to realize the separation of fluorite from calcite in the presence of Ca2+ when using TA as a depressant. Therefore, flotation tests, zeta potential measurements, and adsorption experiments were employed to elucidate the effect of calcium ions on the fluorite and calcite flotation and the adsorption mechanism of NaOL and TA in this study.

2. Materials and Methods

2.1. Materials and Reagents

Pure fluorite and calcite samples (each 5 kg) were obtained through hand picking from the faces of a fluorite mine in Guangxi, China. X-ray diffraction analyses were carried out on D8 Advance Bruker (Bruker Co., Berlin, German)with Cu Kα radiation. The XRD results revealed that the purity of fluorite and calcite is greater than 95%, as shown in Figure 1 and Figure 2. The samples were crushed with a hammer, ground in a laboratory porcelain mill, and then screened to collect −74 + 44 μm particle size fractions for flotation tests and adsorption experiments. Samples further ground to −5 μm in an agate mortar were used for zeta potential measurements.
Chemically pure reagents were obtained from the following sources: Sodium oleate (NaOL) and tannic acid (TA) collected from Aladdin Biological Technology Ltd. (Shanghai, China) were used as a collector and a depressant, respectively. CaCl2 collected from Baisaiqin Chemical Technology Co., Ltd. (Shanghai, China) was used to adjust the ions concentration in the solution. The pH was adjusted with NaOH or HCl stock solutions. Deionized water was used for all experiments.

2.2. Flotation Tests

Flotation was performed in a 150 mL mechanical flotation cell at 1400 rpm with an airflow rate of 0.125 L/min. Fluorite or calcite single mineral (5 g) was combined with 120 mL DI water and mixed for 1 min. NaOH solution was then added to adjust pH 9.0, at which fluorite and calcite may be floated with sodium oleate. This pH was maintained throughout the flotation process. The depressant (TA) was added and conditioned over 2 min after the pH adjustment. Then the collector (NaOL) was added, and the suspension was agitated for further 2 min; the froth collection was performed for 8 min finally. When CaCl2 was used, it was added prior to the pH adjustment and conditioned for 2 min.
For individual mineral flotation, both the floated and unfloated particles were collected, dried, and weighed to calculate the flotation recovery. Repeat tests were carried out for each flotation 3 times, and the average results are reported as the final values.

2.3. Zeta Potential Measurements

The zeta potential of fluorite and calcite were measured at 25 °C using ZetaPlus Zeta Potential Analyzer (Brookhaven Instruments, Austin, TX, USA). All mineral samples were ground to −5 μm by an agate mortar. A total of 20 mg ground sample combined with 50 mL DI water was stirred for 2 min. Then the given pH and reagents concentration was added to the solution in the same order in the flotation test. After allowing the suspension to stir and settle, the zeta potential measurement was performed after transferring the supernatant liquor into a Tiselius cell in a ZetaPlus Unit. For each zeta potential measurement, three tests were repeated, and the average zeta potential was reported.

2.4. Adsorption Experiments

In this study, total organic carbon (TOC) measurement was introduced to evaluate the NaOL concentration before and after the adsorption in the solution. The adsorption experiment of minerals without TA treatment was conducted as follows: Fluorite or calcite sample (1 g) was added to 50 mL DI water at pH 9.0 in a beaker and agitated for 5 min by a magnetic stirrer. Then NaOL solution of a known concentration was added and conditioned for further 15 min. The solid particles were separated by centrifugation for 30 min at 3000 r/min. The concentration of reagents in the supernatant was measured using Elementar liquid TOCII (Elementar Co., Hesse, Germany).
The adsorption experiment of minerals treated with TA was conducted as follows: Fluorite or calcite (1 g) was placed in a beaker and dispersed in 50 mg/L TA solution at pH 9.0 for 30 min. Then, the TA-treated fluorite and calcite samples were obtained after filtering and drying at room temperature. Next, those samples with various amounts of NaOL were added to the DI water or 15 mg/L CaCl2 solution, and the suspension was agitated for further 15 min. All other conditions were the same as those in the adsorption experiment above. The adsorbed amount of collector was then calculated from the difference between the initial (known) concentration and the equilibrium (measured) concentration.
1 g fluorite or calcite in 50 mL DI water at pH 9.0 was used as a blank sample. NaOL dissolved in DI water at pH 9.0 was used to establish the calibration curve. Each adsorption test was repeated three times, and the average was reported in this study.

3. Results and Discussion

3.1. Microflotation Tests

3.1.1. Effect of the NaOL and TA Concentration on the Fluorite and Calcite Flotation

The flotation behavior of fluorite and calcite with various NaOL concentrations at pH 9 is given in Figure 3. The flotation recovery of the two minerals increased gradually with increasing the concentration of NaOL. In the absence of TA, fluorite and calcite exhibited good flotation behavior with 94.8% and 92.6% recovery, respectively, at 150 mg/L NaOL. In addition, the flotation recovery of fluorite was much higher than calcite when the NaOL concentration was below 90 mg/L, and the gap between these two minerals decreases as the NaOL concentration increases. There is no significant difference in flotation recovery between fluorite and calcite at high NaOL concentrations. The results reveal that NaOL has a good adsorption effect on both minerals in alkaline solution [10]. Further, the flotation of fluorite can be achieved at low NaOL concentration due to the stronger chemisorption and the monolayer coverage between RCOO and Ca2+ on the fluorite surface [5,21]. At a higher concentration of NaOL, the physical adsorption of calcium oleate colloids may play a significant role in calcite flotation [22].
Figure 4 shows the flotation recovery of fluorite and calcite with 150 mg/L NaOL as a function of TA concentrations at pH 9. In the presence of TA, calcite recovery decreased dramatically from 92.6% to 13.8%, and fluorite recovery decreased slightly from 94.8% to 72% as the TA concentration increased in the range from 0–50 mg/L, which is necessary for their separation. From the literature, TA has little effect on the chemisorption of NaOL at the fluorite surface while selectively depressing calcite via weakened the adsorption of NaOL on the calcite surface [1]. However, the separation of fluorite and calcite could be changed by the components dissolved from semi-soluble Ca-bearing minerals. Therefore, the effect of calcium ions on the flotation of two minerals was further examined in this work.

3.1.2. Effect of Calcium Ion on Fluorite and Calcite Flotation

Fluorite and calcite flotation were conducted in the presence and absence of 40 mg/L TA as a function of CaCl2 concentration, and the results are shown in Figure 5. The flotation recovery of the two minerals remains constant at approximately 93% without TA in the CaCl2 concentration range of 0–15 mg/L with 150 mg/L NaOL at pH 9. In the presence of TA, the flotation recovery of fluorite reduced from 72% to 16.2% when CaCl2 concentration increased from 0 to 6.0 mg/L. with a further increase in CaCl2 concentration, this decrease slowed down with a 3% recovery at 15 mg/L CaCl2 concentration. Meanwhile, the calcite recovery was low, and the floatability of calcite was hardly affected by adding CaCl2 in the presence of TA. Consequently, this phenomenon reveals that it is impossible to separate fluorite from calcite using NaOL as a collector and TA as a depressant in the presence of calcium ions. From this result, it is apparent that the adsorption of NaOL and TA on the fluorite surface may be different in the presence of calcium ions. In DI water, the preferential adsorption of NaOL takes place on the fluorite surface rather than TA, which may explain the limited inhibition of fluorite flotation by TA [1]. With the addition of CaCl2, NaOL was consumed to generate calcium oleate colloids with Ca2+ in the solution instead of chemisorption on the fluorite surface [19,23]. The physical adsorption between calcium oleate colloids and fluorite surface maintains the floatability of fluorite without TA. However, the TA may have stronger competitive adsorption with fluorite surface than the calcium oleate colloids, and the fluorite could be depressed by TA. This is supported by the flotation test above.

3.1.3. Eliminating the Negative Effect of Ca2+ by Increasing the Dosage of NaOL

The float abilities of fluorite and calcite with massive NaOL concentration in the presence of 15 mg/L CaCl2 and 50 mg/L TA are shown in Figure 6. It is clear that the fluorite recovery was remarkably improved from approximately 3% to 91.4%, with increasing NaOL concentration from 150 mg/L to 300 mg/L. Thereafter, the recovery increased slightly. This result indicates that TA adsorbed on the fluorite surface could be replaced by the excessive NaOL after precipitating Ca2+ in solution due to the stronger attractive interaction of NaOL on the fluorite than that of TA [11]. In the case of calcite flotation, calcite recovery remains low with the increased NaOL concentration. This may attribute to the high-concentration Ca2+ produced by the addition of CaCl2 and calcite dissolution, thereby causing the formation of calcium oleate from NaOL in solution [5,24]. Thus, TA prevents the adsorption of calcium oleate on the calcite surface and inhibits calcite flotation. Based on the flotation test, it suggests that the negative effect of Ca2+ on fluorite flotation could be eliminated by increasing the dosage of NaOL. These findings have been applied in the fifth cleaning flotation flowsheet of a fluorite mine in Guangxi, China. The total consumption of NaOL increased by 7%, approximately, and the flotation recovery of fluorite has improved by nearly 5%, which shows good economic benefits and industrial application value. The interaction of TA and NaOL on the mineral surfaces in the presence and absence of Ca2+ was investigated in the following section.

3.2. Zeta Potential Measurements

In order to understand the adsorption mechanism of NaOL and TA on the mineral surfaces in the presence of Ca2+, the zeta potential was measured, and the results are shown in Figure 7 and Figure 8. Figure 7 shows the zeta potential of fluorite treated and not treated with TA and NaOL as a function of pH in the absence and presence of Ca2+. As can be seen, the isoelectric point of fluorite without any reagents is around pH 6.5, which is close to the reported values in previous studies [25]. The zeta potential of fluorite towards the negative values in the presence of NaOL or TA. The reduced values of NaOL are much larger than that of TA, demonstrating that strong adsorption of NaOL occurs on the fluorite surface. Moreover, a similar zeta potential decrease was observed for fluorite treated with TA followed by NaOL or just NaOL, so it is indicated that the adsorption of NaOL on fluorite surfaces cannot be prevented by TA. This is consistent with the flotation test of fluorite above. When calcium ion was added, the zeta potential of fluorite was close to that with TA alone, suggesting that TA played a dominant role on the fluorite surface under the condition of 15 mg/L CaCl2 and 150 mg/L NaOL. After increasing the concentration of NaOL to 300 mg/L, the decrease in Zeta potential of fluorite occurred, and the values trended the same with the NaOL alone in the range of pH from 3–10, illustrating that TA is possible desorbed and replaced by excess NaOL from the fluorite surface due to strong chemical adsorption between RCOO and Ca2+ on the fluorite surface [16]. The results are correlated well with the fluorite flotation, suggesting that the effect of Ca2+ on fluorite flotation can be mitigated using a massive NaOL collector.
Figure 8 shows the modification of zeta potential on calcite treated with different reagents as the function of pH. Obviously, calcite becomes highly negatively charged in the presence of reagents. Moreover, a larger negative shift of the zeta potential values of calcite was observed with TA than with just NaOL, indicating that the selective adsorption of TA was generated on the calcite surface. When TA was added prior to NaOL, the zeta potential of calcite was close to that of TA alone, which means the depressant TA can also adsorb on the calcite surface in the presence of NaOL. This result is in accordance with Yuehua Hu [1]. With the addition of Ca2+, the zeta potential of calcite remains at the negative values, which is similar to the TA alone. In addition, no evident change was observed in the zeta potential of calcite with 150 mg/L NaOL or 300 mg/L NaOL. This result demonstrates that some preferential adsorption sites for TA always exist on the calcite surface.

3.3. Adsorption Mechanism Study

The adsorption of NaOL on the fluorite and calcite under different conditions is shown in Figure 9 and Figure 10. Figure 9 shows the adsorption isotherms of NaOL on fluorite treated or not treated with TA in the absence and presence of Ca2+. As can be seen, the adsorbed amount of NaOL on the fluorite surface increased gradually with its initial concentrations increased. In the absence of Ca2+, the fluorite surface could be effectively coated with NaOL species. In addition, only a small decrease in NaOL adsorption was found on the fluorite surface with TA treatment, which demonstrates that the stronger chemisorption of NaOL was bonded with the calcium site at the fluorite surface rather than TA. In the presence of Ca2+, a reduction in NaOL adsorption amount on the TA-treated fluorite surface was observed with the NaOL concentration below 150 mg/L, while the gradually increasing trend occurred in the range of NaOL concentration from 200 mg/L to 300 mg/L. It is documented that the calcium ion dominates the surfactant adsorption mechanism at the Ca-bearing mineral surface [16]. In this study, the addition of Ca2+ interacts with the NaOL by forming calcium oleate through carboxylate reactions in the bulk solution, which change the NaOL adsorption mechanism from the chemisorption to the precipitation of calcium oleate collides on the fluorite surface [20]. TA can prevent this physical adsorption of calcium oleate and depress the fluorite with the NaOL concentration below 150 mg/L. With the increase in NaOL centration, the excess NaOL reabsorb on the fluorite surface after consuming the Ca2+ in the solution and then improves the fluorite flotation. This result is consistent with the flotation test shown in Figure 6.
The adsorption isotherms of NaOL on calcite treated or not treated with TA in the absence and presence of Ca2+ are given in Figure 10. The trend observed for the adsorption of NaOL on calcite was similar to this for fluorite without TA and Ca2+, as the amount of NaOL adsorbed on calcite was enhanced by increasing their initial concentration. The relatively high NaOL adsorption on the calcite surface may be related to the high concentration of Ca2+ dissolved from calcite, thereby causing the physical adsorption of calcium oleate colloids and achieving calcite flotation [24]. Nevertheless, the amount of NaOL adsorbed on the calcite surface after TA treatment was much less in the presence or absence of Ca2+ even at the high NaOL concentration, suggesting TA cannot be desorbed from the calcite surface. Therefore, the separation of fluorite from calcite could be achieved under the condition of high NaOL concentration using TA as a depressant.

4. Conclusions

In this study, calcium ion has been shown to exhibit a significant impact on fluorite recovery. Flotation experiments illustrate that fluorite and calcite exhibit good floatability with NaOL. TA is an effective depressant for calcite but exerts little influence on fluorite flotation in deionized water. With the addition of Ca2+, fluorite flotation recovery decreased dramatically in the presence of TA. Then, the fluorite flotation can also be recovered by increasing the NaOL concentration. Adsorption tests and zeta potential results consistently showed that TA has little effect on the chemisorption of NaOL on the fluorite surface. However, the adsorption of NaOL on the fluorite surface was strongly weakened in the presence of Ca2+ and TA at the same time, which caused the problem of the separation of fluorite from calcite. This negative effect of Ca2+ can be removed by raising the NaOL concentration, suggesting that excessive NaOL can reabsorb on the fluorite surface and then improve its flotation. On the other side, TA always occupies the site of the calcite surface and depresses the calcite flotation in this study, which provides a possibility of separating fluorite from calcite in a calcium species contained solution using high NaOL concentration as a collector and TA as a depressant. These findings also emphasize that it is necessary to consider the inhibition effects and selective adsorption mechanisms of dissolved components from semi-soluble minerals on the mineral surfaces.

Author Contributions

Formal analysis, Y.Q.; investigation, X.Q. and B.C.; methodology, Y.H.; resources, T.S. and Z.W.; writing-original draft, Y.Q.; writing-review and editing, Y.H. and Y.Q.; project administration, Y.Q. and T.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by National Natural Science Foundation of China (No. 51504173).

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zhang, C.; Wei, S.; Hu, Y.; Tang, H.; Gao, J.; Yin, Z.; Guan, Q. Selective adsorption of tannic acid on calcite and implications for separation of fluorite minerals. J. Colloid Interface Sci. 2018, 512, 55–63. [Google Scholar] [CrossRef] [PubMed]
  2. Gao, Y.; Gao, Z.; Sun, W.; Hu, Y. Selective flotation of scheelite from calcite: A novel reagent scheme. Int. J. Miner. Process. 2016, 154, 10–15. [Google Scholar] [CrossRef]
  3. Rao, K.H.; Antti, B.M.; Forssberg, E. Mechanism of oleate interaction on salt-type minerals part I. Adsorption and electrokinetic studies of calcite in the presence of sodium oleate and sodium metasilicate. Colloids Surf. 1988, 34, 227–239. [Google Scholar] [CrossRef]
  4. Rao, K.H.; Antti, B.M.; Forssberg, E. Mechanism of oleate interaction on salt-type minerals, Part II. Adsorption and electrokinetic studies of apatite in the presence of sodium oleate and sodium metasilicate. Int. J. Miner. Process. 1990, 28, 59–79. [Google Scholar] [CrossRef]
  5. Pugh, R.; Stenius, P. Solution chemistry studies and flotation behaviour of apatite, calcite and fluorite minerals with sodium oleate collector. Int. J. Miner. Process. 1985, 15, 193–218. [Google Scholar] [CrossRef]
  6. Free, M.L.; Miller, J.D. The significance of collector colloid adsorption phenomena in the fluorite/oleate flotation system as revealed by FTIR/IRS and solution chemistry analysis. Int. J. Miner. Process. 1996, 48, 197–216. [Google Scholar] [CrossRef]
  7. Karlkvist, T.; Patra, A.; Rao, K.H.; Bordes, R.; Holmberg, K. Flotation selectivity of novel alkyl dicarboxylate reagents for apatite-calcite separation. J. Colloid Interface Sci. 2015, 445, 40–47. [Google Scholar] [CrossRef]
  8. Zhang, W.; Honaker, R.Q.; Groppo, J.G. Flotation of monazite in the presence of calcite part I: Calcium ion effects on the adsorption of hydroxamic acid. Miner. Eng. 2017, 100, 40–48. [Google Scholar] [CrossRef]
  9. Zhang, Z.; Wang, B.; Fu, J. Influence of the mutual transformation of mineral surfaces on the flotation of salt type mineral coexistence system. Met. MINE 1995, 226, 38–41. [Google Scholar]
  10. Gao, Z.; Bai, D.; Sun, W.; Cao, X.; Hu, Y. Selective flotation of scheelite from calcite and fluorite using a collector mixture. Miner. Eng. 2015, 72, 23–26. [Google Scholar] [CrossRef]
  11. Hernáinz Bermúdez de Castro, F.; Calero de Hoces, M. Influence of quebracho and sodium silicate on flotation of celestite and calcite with sodium oleate. Int. J. Miner. Process. 1993, 37, 283–298. [Google Scholar] [CrossRef]
  12. Zhou, H.; Zhang, Y.; Tang, X.; Cao, Y.; Luo, X. Flotation separation of fluorite from calcite by using psyllium seed gum as depressant. Miner. Eng. 2020, 159, 106514. [Google Scholar] [CrossRef]
  13. Cui, Y.; Jiao, F.; Wei, Q.; Wang, X.; Dong, L. Flotation separation of fluorite from calcite using sulfonated lignite as depressant. Sep. Purif. Technol. 2020, 242, 116698. [Google Scholar] [CrossRef]
  14. Gao, J.; Hu, Y.; Sun, W.; Liu, R.; Gao, Z.; Han, H.; Lyu, F.; Jiang, W. Enhanced separation of fluorite from calcite in acidic condition. Miner. Eng. 2019, 133, 103–105. [Google Scholar] [CrossRef]
  15. Zhang, Z.; Cao, Y.; Sun, L.; Ma, Z.; Liao, Y. Interaction forces between scheelite and fluorite in calcium solution measured by atomic force microscopy. Appl. Surf. Sci. 2019, 486, 323–336. [Google Scholar] [CrossRef]
  16. Fa, K.; Nguyen, A.V.; Miller, J.D. Interaction of calcium dioleate collector colloids with calcite and fluorite surfaces as revealed by AFM force measurements and molecular dynamics simulation. Int. J. Miner. Process. 2006, 81, 166–177. [Google Scholar] [CrossRef]
  17. Amankonah, J.O.; Somasundaran, P. Effects of dissolved mineral species on the electrokinetic behavior of calcite and apatite. Colloids Surf. 1985, 15, 295–307. [Google Scholar] [CrossRef]
  18. Young, C.A.; Miller, J.D. Effect of temperature on oleate adsorption at a calcite surface: An FT-NIR/IRS study and review. Int. J. Miner. Process. 2000, 58, 331–350. [Google Scholar] [CrossRef]
  19. Dong, L.; Zhu, H.; Jiao, F.; Qin, W.; Jia, W. Effect of calcium ions on scheelite flotation using mixed collectors. Sep. Sci. Technol. 2019, 54, 153–162. [Google Scholar] [CrossRef]
  20. Zhang, Z.; Cao, Y.; Ma, Z.; Liao, Y. Impact of calcium and gypsum on separation of scheelite from fluorite using sodium silicate as depressant. Sep. Purif. Technol. 2019, 215, 249–258. [Google Scholar] [CrossRef]
  21. Hu, J.S.; Misra, M.; Miller, J.D. Characterization of adsorbed oleate species at the fluorite surface by FTIR spectroscopy. Int. J. Miner. Process. 1986, 18, 73–84. [Google Scholar] [CrossRef]
  22. Yalamanchili, M.R.; Kellar, J.J.; Miller, J.D. Adsorption of collector colloids in the flotation of alkali halide particles. Int. J. Miner. Process. 1993, 39, 137–159. [Google Scholar] [CrossRef]
  23. Fa, K.; Jiang, T.; Nalaskowski, J.; Miller, J.D. Interaction forces between a calcium dioleate sphere and calcite/fluorite surfaces and their significance in flotation. Langmuir 2003, 19, 10523–10530. [Google Scholar] [CrossRef]
  24. Zhu, H.; Qin, W.; Chen, C.; Chai, L.; Jiao, F.; Jia, W. Flotation separation of fluorite from calcite using polyaspartate as depressant. Miner. Eng. 2018, 120, 80–86. [Google Scholar] [CrossRef]
  25. Severov, V.; Filippov, L.; Filippova, I. Interrelation of site population of calcic amphiboles with their electrochemical and flotation properties. In Proceedings of the IMPC 2014—27th International Mineral Processing Congress, Santiago, Republic of Chile, 20 October 2014. [Google Scholar]
Figure 1. XRD spectra of fluorite samples used for flotation tests.
Figure 1. XRD spectra of fluorite samples used for flotation tests.
Minerals 12 00996 g001
Figure 2. XRD spectra of calcite samples used for flotation tests.
Figure 2. XRD spectra of calcite samples used for flotation tests.
Minerals 12 00996 g002
Figure 3. Effect of NaOL concentration on the flotation recovery of fluorite and calcite.
Figure 3. Effect of NaOL concentration on the flotation recovery of fluorite and calcite.
Minerals 12 00996 g003
Figure 4. Effect of TA concentration on the flotation recovery of fluorite and calcite.
Figure 4. Effect of TA concentration on the flotation recovery of fluorite and calcite.
Minerals 12 00996 g004
Figure 5. Effect of Ca2+ concentration on the flotation of fluorite and calcite in the presence and absence of TA.
Figure 5. Effect of Ca2+ concentration on the flotation of fluorite and calcite in the presence and absence of TA.
Minerals 12 00996 g005
Figure 6. Effect of NaOL concentration on the flotation of fluorite and calcite in the presence of Ca2+ and TA.
Figure 6. Effect of NaOL concentration on the flotation of fluorite and calcite in the presence of Ca2+ and TA.
Minerals 12 00996 g006
Figure 7. Effect of the addition of different reagents on the zeta potentials of fluorite (TA = 50 mg/L, NaOL = 150 mg/L, NaOL’ = 300 mg/L, CaCl2 = 16 mg/L).
Figure 7. Effect of the addition of different reagents on the zeta potentials of fluorite (TA = 50 mg/L, NaOL = 150 mg/L, NaOL’ = 300 mg/L, CaCl2 = 16 mg/L).
Minerals 12 00996 g007
Figure 8. Effect of the addition of different reagents on the zeta potentials of Calcite (TA = 50 mg/L, NaOL = 150 mg/L, NaOL’ = 300 mg/L, CaCl2 = 16 mg/L).
Figure 8. Effect of the addition of different reagents on the zeta potentials of Calcite (TA = 50 mg/L, NaOL = 150 mg/L, NaOL’ = 300 mg/L, CaCl2 = 16 mg/L).
Minerals 12 00996 g008
Figure 9. Adsorption isotherms of NaOL on fluorite treated or not treated with TA in the absence and presence of Ca2+.
Figure 9. Adsorption isotherms of NaOL on fluorite treated or not treated with TA in the absence and presence of Ca2+.
Minerals 12 00996 g009
Figure 10. Adsorption isotherms of NaOL on calcite treated or not treated with TA in the absence and presence of Ca2+.
Figure 10. Adsorption isotherms of NaOL on calcite treated or not treated with TA in the absence and presence of Ca2+.
Minerals 12 00996 g010
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Qian, Y.; Qiu, X.; Shen, T.; Huai, Y.; Chen, B.; Wang, Z. Effect of Calcium Ion on the Flotation of Fluorite and Calcite Using Sodium Oleate as Collector and Tannic Acid as Depressant. Minerals 2022, 12, 996. https://doi.org/10.3390/min12080996

AMA Style

Qian Y, Qiu X, Shen T, Huai Y, Chen B, Wang Z. Effect of Calcium Ion on the Flotation of Fluorite and Calcite Using Sodium Oleate as Collector and Tannic Acid as Depressant. Minerals. 2022; 12(8):996. https://doi.org/10.3390/min12080996

Chicago/Turabian Style

Qian, Yupeng, Xuan Qiu, Tiewei Shen, Yangyang Huai, Bin Chen, and Zhen Wang. 2022. "Effect of Calcium Ion on the Flotation of Fluorite and Calcite Using Sodium Oleate as Collector and Tannic Acid as Depressant" Minerals 12, no. 8: 996. https://doi.org/10.3390/min12080996

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop