Next Article in Journal / Special Issue
Fe-Substitution for Ni in Misch Metal-Based Superlattice Hydrogen Absorbing Alloys—Part 2. Ni/MH Battery Performance and Failure Mechanisms
Previous Article in Journal / Special Issue
Increase in the Surface Catalytic Ability by Addition of Palladium in C14 Metal Hydride Alloy
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Review

C14 Laves Phase Metal Hydride Alloys for Ni/MH Batteries Applications

1
Department of Chemical Engineering and Materials Science, Wayne State University, Detroit, MI 48202, USA
2
BASF/Battery Materials—Ovonic, 2983 Waterview Drive, Rochester Hills, MI 48309, USA
3
Department of Mechanical Engineering, Wayne State University, Detroit, MI 48202, USA
4
Department of Chemical Engineering and Materials Science, Michigan State University, East Lansing, MI 48824, USA
*
Author to whom correspondence should be addressed.
Batteries 2017, 3(3), 27; https://doi.org/10.3390/batteries3030027
Submission received: 6 June 2017 / Revised: 16 August 2017 / Accepted: 18 August 2017 / Published: 14 September 2017
(This article belongs to the Special Issue Nickel Metal Hydride Batteries 2017)

Abstract

:
C14 Laves phase alloys play a significant role in improving the performance of nickel/metal hydride batteries, which currently dominate the 1.2 V consumer-type rechargeable battery market and those for hybrid electric vehicles. In the current study, the properties of C14 Laves phase based metal hydride alloys are reviewed in relation to their electrochemical applications. Various preparation methods and failure mechanisms of the C14 Laves phase based metal hydride alloys, and the influence of all elements on the electrochemical performance, are discussed. The contributions of some commonly used constituting elements are compared to performance requirements. The importance of stoichiometry and its impact on electrochemical properties is also included. At the end, a discussion section addresses historical hurdles, previous trials, and future directions for implementing C14 Laves phase based metal hydride alloys in commercial nickel/metal hydride batteries.

1. Introduction

Nickel/metal hydride (Ni/MH) batteries have a wide range of applications including portable consumer electronics [1], transportation [2], and stationary power sources [3,4] as it features benefits such as safe chemistry, sustainable life, a stable raw material supply, high performance, and reasonable cost [5]. The most common metal hydride (MH) alloy used as the active material in negative electrode of Ni/MH batteries is a misch-metal (combination of La, Ce, Pr, and Nd) based AB5 alloy with a CaCu5 crystal structure. Recently, a misch-metal and Mg in the superlattice alloy (A2B7 type) with its corresponding improvement in the gravimetric energy density has become more popular in consumer and stationary applications [5,6,7,8,9]. Meanwhile, the Laves phase AB2 MH alloy has also been proposed to improve the energy density of Ni/MH batteries. Although the AB2 MH alloy has the potential for relatively high capacity potential (440 mAh·g−1 [10,11] when compared to 330 mAh·g−1 from the AB5 alloy), it suffers from a relatively slow electrochemical reaction rate and a less-desirable cycle life (see comparison in Table 1) [12]. A further comparison of the main battery performances between AB2 and AB5 MH alloys can be found in previous research (Table 1 in [13]). Numerous papers, including a few reviews [14,15,16,17,18,19,20], have been have examined how to improve the electrochemical properties of AB2 MH alloys, however, an updated comprehensive review of this subject would be of use. The current work details the alloy preparation methods, performance requirements, failure mechanisms, constituent phases, selection of elements and stoichiometry, as well as the historical challenges and directions for future research.
C14, C15, and C36 Laves phases are composed of the same A2B4 unit-block, but with different stacking sequences; C14 has an a-b-a-b stacking sequence, which leads to a hexagonal structure (Figure 1a); C15 has an a-b-c-a-b-c stacking and a cubic structure (Figure 1b); and C36 exhibits a-b-a-c stacking and a rhombohedral (dihexagonal) structure (Figure 1c) [21,22,23]. The C14 and C15 phases are more commonly observed in MH alloys, whereas the C36 phase may exist between the C14 and C15 phases [24] but is difficult to identify using X-ray diffraction (XRD) [25,26]. Alloys with both C14 and C15 crystal structures serve as hydrogen-storage (H-storage) alloys and electrode materials. C15 alloys have better high-rate and low-temperature performance, however the C14 alloys were more widely used earlier when alloy composition design was driven by capacity and cycle stability. An AB2 MH alloy with a C14-predominated structure was used in the first commercialized electric vehicle, EV1 by General Motor (Detroit, MI, USA). Similar alloys with the same structure were also used in the first-generation Ni/MH batteries made by Gold Peak Industries (Hong Kong, China) and Hitachi-Maxwell (Osaka, Japan). Recently, the electrochemical performances of a state-of-art C14-predominate MH alloy were compared to those from a recently proposed C15-based MH alloy together with a review of the development works done on the C15-based MH alloys [27]. In this paper, we will review only research focused on the C14-predominated MH alloys.

2. Alloys Preparation

Conventionally, when used as the active material in negative electrodes of Ni/MH batteries, the MH alloys are initially prepared by melting and casting. Then, an annealing process is applied to the ingot to improve compositional uniformity and to reduce internal stress. To reach a final particle size of less than 200 mesh (75 µm), most ingots need to be crushed into powder through mechanical grinding or hydrogenation. The powder may require additional surface treatments to enhance its electrochemical properties. Negative electrode fabrication methods have been previously reviewed [13].

2.1. Melting and Casting

A few preparation methods for MH alloys are described in an introductory article [29] that covers conventional vacuum induction melting (VIM) [30], arc melting (AM) [31], centrifugal casting (CC), melt-spinning (MS) [32,33,34], gas atomization (GA) [35,36], and mechanical alloying (MA) [37,38,39]. A vacuum plasma spray (PS) has also been employed for research purposes [40]. While AM only produces small quantity of alloy (5 to 200 g) for laboratory use, VIM can produce ingots ranging from 1 kg to 1 ton (Figure 2). In terms of electrochemical property, no distinct difference is observed between AB2 MH alloys prepared by VIM and those prepared by AM [41], except for a slightly higher capacity obtained from VIM due to a larger sample/chamber ratio [42]. Samples from different locations of a VIM-process ingot may have different microstructures, but the electrochemical capacities are very similar. For example, the microstructures of different pieces of ingot prepared by a 60-kg VIM furnace are shown in Figure 3. According to the analytic results from x-ray diffraction (X'Pert Pro, Philips, Amsterdam, The Netherlands) and scanning electron microscope (SEM) (JEOL-JSM6320F, JEOL, Tokyo, Japan) with the x-ray energy dispersive spectroscopy capability, this alloy is C14-predominant with C15, TiNi, and families of (Zr, Ni) secondary phases. We obtained this composition by continuing optimization and testing more than 400 alloys. The properties of C14-predominated alloys prepared by VIM and other techniques were also previously compared [43] and are summarized in Table 2. Because of the small sample size, use of expensive argon gas, and high utility costs from water chiller and arc power supply, AM is the most expensive method for making MH alloys. Photographs of equipment and different pouring processes are shown in Figure 4 and Figure 5, respectively. SEM surface morphology and cross-section micrographs of products are compared in Figure 6 and Figure 7, respectively. A review of Japanese Patent Applications shows 9 different ingot preparation methods for MH alloys [44]. For MH alloys that are sensitive to oxygen contamination from the reduction of ceramic refractory used as furnace crucible, a skull VIM melting can be used (Figure 8). MA in a shaker mill or an attritor is a popular method for making meta-stable/amorphous alloys not allowed in the phase diagram [45] (Figure 9).

2.2. Particle Size Reduction

Particle size influences capacity and high-rate dischargeability (HRD) behavior, but not activation properties [46]. As such, a proper particle size is required for battery operation. Unlike the conventional jar crusher used for AB5 MH alloys, the high hardness of C14 MH alloys requires a hydrogenation process to create fissures and cracks for further grinding [47]. A stationary hydrogen reactor for laboratory use (2-kg load), a prototype rotational hydrogen reactor (50 kg), and a mass production stationary hydrogen reactor (5 tons) are shown in Figure 10. Operation details for the stationary and rotational hydrogen reactors can be found in the associated U.S. Patents [48,49]. Further reduction to a desirable size can be achieved by crushing [50], dry ball milling [51], wet ball milling [52], centrifugal grinding, or jet milling [53]. Three different powder fabrication methods—hydrogenation, dry ball milling, and wet ball milling—on a F-treated AB2 MH alloy, were compared and the third showed the best electrochemical performance [54].

2.3. Annealing

The main purpose of annealing is to improve uniformity in both composition and micro-structure. Annealing is a necessary step to prepare commercial grade AB5 MH alloys with a long cycle life [55] (Figure 11a,b). In the case of AB2 MH alloys, non-Laves secondary phases improve the electrochemical properties of an alloy [56] through synergetic effects [57] and are diminished by annealing treatments [58,59,60,61]. Therefore, annealing is not required for AB2 MH alloys, except for those prepared by GA and with a surface oxide layer, which can be reduced to the metallic state by annealing in hydrogen [62] (Figure 11c). Annealing in Ar was also improved the capacity of GA- [63] and MS- [64] produced AB2 MH alloys because of the ability to increase the surface crystallinity. The positive contribution of thermal annealing to electrochemical capacity was previously reported by Klein et al. [65].

2.4. Surface Treatment

Various surface treatments are available for AB2 MH alloys. A fluorination process can improve the surface anti-corrosion capability [66,67,68,69,70,71] and HRD [72], while a hot alkaline bath helps remove the native oxide that forms during the processes and creates a less dense oxide with catalytic Ni, which further increases the surface’s catalytic ability [51,66,73,74] and HRD [72]. Other methods include hot-charging performed at 80 °C [75], surface treatment in NH4F and NiCl2 solution [76], NiO coating by the sol-gel method [77], electroless Cu-coating [78], ball-milling with [79,80] or without Ni powder [81,82], ball-milling with La-containing AB5 or A2B7 MH alloys [83], and surface reduction by KBH4 and NaBH4 [84].

3. Performance Criteria

The general requirements for an MH alloy that is suitable for use as the negative electrode in Ni/MH batteries include high electronic conductivity, a durable anti-corrosion surface, high H-storage capability, fast bulk hydrogen diffusibility, adequate metal-hydrogen (M-H) bond strength, acceptable cost, small lattice expansion during hydrogenation, and environmental friendliness [85,86]. As the applications of Ni/MH batteries become more versatile, the demands of MH alloys also vary. We classify the prerequisites of specific alloy properties in accordance with application in Table 3. For the AB2 MH alloys, the surface catalytic ability is not as good as those in AB5 and A2B7 MH alloys, because of its lower B/A ratio, which contributes to a lower level of metallic Ni on the surface [87]. But the corrosion product of AB2 alloy is dissoluble in electrolyte, which is different from the highly packed oxide of rare earth elements (RE) in AB5 alloys, and makes it a better candidate for high-temperature applications. The small hysteresis found in the pressure-concentration-temperature (PCT) analysis between absorption and desorption isotherm in AB2 reduces the pulverization rate and helps improve cycle stability [88,89].

4. Failure Mechanism

While the failure mechanism of the AB5 MH alloy has been studied extensively and reviewed in detail [90], similar studies on AB2 MH alloys are rare [91,92]. Unlike the surface of AB5 MH alloys, which are covered by an inert layer of La(OH)3 after numerous cycles, the AB2 MH alloy forms soluble complex ions, including HZrO3, HMnO2, and AlO2−., which migrate through the separator into the positive electrode, causing micro-shorts and particle pulverization at the electrodes, which leads to positive electrode failure. The surface passivation of AB5 MH alloys causes stable capacity degradation, while the failure at the positive electrode with AB2 MH alloys creates a pressure increase, cell venting, and a sudden capacity drop near the end of the cycle life (Figure 12). Three AB2 MH alloy degradation modes (oxidation, pulverization, and amorphization) are discussed in this section.

4.1. Oxidation

The activated (alkaline bath treated or cycled) AB2 alloy surface consists of a top non-electrochemical reactive ZrO2 patch, a surface oxide (~200 nm) with embedded metallic Ni/Co-clusters [10,93], and an amorphous buffer layer (~100 nm) underneath [94]. In one example, the Zr/Ti ratios are 8.2, 1.2, 0.8, and 1.9 for the top oxide, supporting oxide, buffer oxide, and bulk, respectively, which indicates a higher leaching rate for Zr compared to that of Ti [94]. The metallic inclusions on the surface of the AB2 alloy were thought to be vital for the surface electrochemical reaction until it was determined that electrolyte-conducting channels coated with catalysts on the surface of the inner side of the alloy bulk can significantly improve low-temperature performance [95]. The leaching rates of constituent elements from a typical C14 MH alloy are calculated in Table 4 and follow the trend of Al > V > Zr > Ti > Mn. Oxidation and pulverization are the major capacity degradation mechanisms for AB2 MH alloys [96,97].

4.2. Pulverization

Particle pulverization is a key failure mode for AB2 MH alloys, because it increases the surface area of the electrode, which leads to more severe oxidation [98]. High internal stress exists in AB2 MH alloy after hydrogenation, and cannot be removed by annealing because of the beneficial multi-phase structure. Thus, the initial pulverization due to the internal stress in AB2 MH alloys is more severe than that in AB5 MH alloys. But, because of the synergetic effect between the main storage phase and the catalytic secondary phase, the PCT hysteresis (the main reason for pulverization during hydride/dihydride cycling) in AB2 is much smaller than that in AB5 and, thus, a small degree of pulverization during cycling is expected from AB2. Two SEM micrographs showing the pulverizations after activation (10 cycles) and near the end of cycle life (450 cycles) are presented in Figure 13. Interestingly, a V-free AB2 MH alloy also shows a higher pulverization rate than a V-containing alloy [92].

4.3. Amorphization

Hydrogen-induced-amorphization (HIA) frequently occurs on AB2 alloys [99,100], especially those with an atomic radius ratio between A- and B-site atoms (RA/RB) > 1.37 [101]. The amorphous alloy may have a lower electrochemical capacity [101,102] but better HRD [103,104] compared to its crystalline counterpart. An amorphous C14 MH alloy went through MA and its capacity decreased from 325 to 25 mAh·g−1 [105]. A similar degradation of capacity caused by amorphization from MS has been previously reported [64].

5. Non-Laves Secondary Phases

During cooling from the liquid, the C14 phase solidifies first, followed by the C15 phase, and then finally a TiNi phase. The TiNi phase further transforms into Zr7Ni10, Zr9Ni11, and ZrNi phases via solid-state reactions [106,107,108,109] (Figure 14). When other modifiers are present, additional secondary phases are also formed. These secondary phases may not store large amounts of hydrogen, but they may improve electrochemical performance through the synergetic effect [57].

5.1. TiNi

A TiNi phase is a commonly observed secondary phase in C14 MH alloys. TiNi has a large soluble Zr content [110]. Occasionally, the Zr-content in the TiNi phase can be larger than the Ti-content [111]. A TiNi phase was found to increase the discharge capacity, and to improve the charge retention and cycle life while lowering HRD capability [56]. In addition, it is known to improve low-temperature kinetics [112,113]. The electrochemical performances of TiNi-based MH alloys were previously reported [114,115,116,117].

5.2. ZrxNiy

Three Zr-dominated secondary phases are commonly seen in C14 MH alloys, specifically ZrNi [30], Zr9Ni11 [65,118], and Zr7Ni10 [118]. ZrNi and Zr7Ni10 phases are found to increase HRD, but sacrifice capacity and cycle stability, while Zr9Ni11 does the opposite [56,119]. Zr7Ni10 gradually shifted to Zr9Ni11 as secondary phases in C14 MH alloys with increasing V-content [120]. The electrochemical properties of ZrNi [30,121,122,123], Zr9Ni11 [121,124,125], Zr7Ni10 [30,121,124,125,126,127], and other Zr8Ni21 [30,121,124,125,128], Zr2Ni7 [30,121,129], and ZrNi5 [130] based MH alloys are also available.

5.3. V-Based bcc Solid Solution

In the MH alloys with a high V-content, a V-based body-centered-cubic (bcc) is commonly observed [131,132,133]. This phase is unlikely to corrode and remains at the surface after activation [72]. As the V-content and the B/A ratio increases, the microstructure of the alloy will change from a predominated Laves phase into a Laves-phase-related bcc two-phase solid solution [134]. The electrochemical storage of the two-phase alloy is higher, but the HRD suffers in the Laves-phase alloy [135].

5.4. ZrO2

ZrO2 is formed during the melting stage and acts as an oxygen scavenger [136], which is ordinarily seen in C14 MH alloys with higher Zr/Ti ratios [111]. It forms a protective barrier against oxidation [72], but does not form hydride under normal operating conditions in batteries [137].

5.5. Other Secondary Phases

Other secondary phases can be detected using non-transition metal modifiers, such as RE. The solubility of RE in the C14 phase is extremely low and the addition of Y, La, Ce, Nd results in the formation of YNi [138], LaNi [139], CeNi [140], and NdNi [141] phases, respectively. These RE-Ni phases are detrimental to the electrochemical performance of MH alloys [112]. Like RE-Ni, the ScNi secondary phase increased discharge capacity, but weakened cycle stability [142]. A combination of hypo-stoichiometry and the addition of RE can boost low-temperature alloy performance [113]. High Mg-content secondary phases have been detected and facilitate the activation process [143,144]. A ZrC phase was formed with a C-addition and improves charge retention but deteriorates cycle life, HRD, and low-temperature performance. Zr2Ni2Sn [56,136] and Zr (Ni, Mn) Sn0.35 [145] phases can be found in alloys with a relatively high Sn-content and are detrimental to the alloys’ electrochemical performance. The structure and properties of Zr2Ni2Sn have been reported [146].

6. Selections of Element

AB2 alloys have a greater compatibility of constituent elements, compared to that of AB5 MH alloys, because of their superb solubility of components and great number of available phases. The compatibility of substituting elements makes AB2 a better candidate to meet various application demands. Laves phase alloys are composed of A-site and B-site atoms (Figure 1). The A-site atom is usually larger than the B-site atom, but tends to shrink as the electronegativity of the B-site atom increases, resulting in electron transfer. The ideal RA/RB is 1.225 [147].

6.1. A-Site Element

For electrochemical applications, Ni, with an atomic radius of 1.377 Å in the Laves phase, is the major B-site element [148], which limits the choice of A-site element to those with an atomic radius of approximately 1.68 Å. Some physical properties of the A-site atoms are summarized in Table 5. Ti and Zr are the most frequently used A-site elements in Laves phase MH alloys because of their availability. Zr has the strongest M-H bond (lowest heat of hydride formation [149]) and the adjustment of Zr/Ti content is the most effective method to change M-H bond strength.

6.1.1. Titanium

Ti results in weaker M-H bond strength, higher PCT equilibrium pressure [65], and improved HRD performance [41,150,151]. Ti forms an inert layer of TiO2 and impedes activation [31,152], which improves cycle stability [153] and causes capacity degradation [154]. However, another group reported that Ti is beneficial for improving activation [155]. Ti-content impacts the discharge capacity in two competing ways: weaker M-H bonds lead to a lower capacity, but higher plateau pressure also improves the reversibility and increases the discharge capacity. Previous research has documented that increasing Ti-content has led to increasing [156,157,158,159], decreasing [155,158,160], and unchanged [150] electrochemical discharge capacities. A high Ti-content also contributes to a higher abundance of bcc phase [161] and a higher C14 abundance [162] because of its higher chemical potential [163].

6.1.2. Zirconium

To maintain stoichiometry in comparison to AB2, the sum of Ti- and Zr-contents is approximately 33 at %. Therefore, Zr has the opposite effects of Ti. A higher Zr-content will stabilize the hydride [163] and lower HRD [150]. The bulk oxide of Zr is usually formed during solidification and has a higher solubility in KOH solution than TiO2 [87]. A dense layer of ZrO2 formed on the surface of the Zr particles during powder processing (grinding, sifting, and packaging), and impedes the activation process [152,164,165].

6.1.3. Hafnium

Not many studies have examined the electrochemical properties of Hf- substituted AB2 MH alloys [42,160]. An XRD study confirms that Hf and Ti share the A-site and V and Ni are found in the B-site [166]. Hf-substitution yields a slightly smaller unit cell [167], which is unexpected because of its relatively large atomic radius (Table 5). The reduced lattice constant c/a ratio with the addition of Hf [167] predicts a lower pulverization rate. Partially substituting Hf for Zr results in a lower electrochemical capacity, but a higher HRD [160].

6.1.4. Niobium

Nb occupying the A-site was confirmed by a Rietveld analysis with XRD data from a substituted ZrCr2 alloy [168]. Partial replacement of Zr by Nb leads to a smaller C14 unit cell volume and, consequently, a higher PCT plateau pressure [169]. It increases the C14 phase abundance and reduces lattice constants [167]. Like Hf, Nb also contributes to a reduced lattice constant c/a ratio [167] leading to a smaller pulverization rate. The NiNb secondary phase is a poor catalyst/H-storage material and, remarkably, reduces the surface exchange current [169]. Like Hf, Nb-substitution deteriorates capacity [42], but enhances HRD [160].

6.1.5. Palladium

Pd is smaller than both Ti and Zr, and when it enters the A-site, it reduces the unit cell of the Laves phases, which results in a decrease in discharge capacity. However, it also enhances the surface catalytic ability and improves both HRD and low-temperature performance for the alloy [170]. Improvement in HRD of C14 alloys was also reported by Yang, Ovshinsky, and their coworkers [171,172].

6.1.6. Scandium

Use of Sc, another expensive additive, in AB2 MH alloy is scarce. The gaseous phase H-storages of C15/C36 ScM2 (M = Fe, Co, and Ni) were reported [173] with an electrochemical study of a C15 ScNiCo0.2Mn0.5Cr0.2 alloy [174]. The partial replacement by Zr and Y in Sc-based C15 showed cycle stability improvement with the corresponding sacrifice in discharge capacity [142]. The addition of Sc increased the abundance of the ZrNi secondary phase, improved the activation and capacity, but resulted in a trade-off in HRD [175].

6.2. B-Site Element

Ni is the most widely used B-site element in alkaline battery applications. However, Ti, Zr, and their mixture do not form Laves phase intermetallic compound (IMC) with Ni [176]. Therefore, B-site substitutions, mainly from the first row of transition metals—because of their availability and light weight—are essential for the stability of Laves phase IMC. Both the electron affinity and the atomic radius decrease as the atomic number of the modifier atom increases, which reduces the average metal-hydrogen bond strength, increases plateau pressure, and decreases H-storage capacity. With different solubility and chemical properties related to corrosion, these modifier elements are crucial for engineering various electrochemical properties and will be reviewed in the following sections. Various properties of the first-row transition metals are summarized in Table 6. The atomic radius of the element decreases as the atomic number increases until Ni and then increases from Cu and Zn. The number of IMC with Ti also increases roughly with increasing atomic number.

6.2.1. Vanadium

V is the only B-site element that brings high H-storage capacity [17]. It results in a more stable hydride, more disorder, but also decreases peak power and charge retention [177]. The high leaching rate of V is the main cause of poor charge retention in conventional V-containing MH alloys [87,178]. The high electronic conductivity of V also improves the activation property of alloys [179]. A balance of V-content is needed to optimize battery performance [180]. V-free MH C14 MH alloys were designed to address the charge retention issue, but did so at the expense of cycle stability [144,178]. The large atomic radius of V enlarges the alloy unit cell and reduces the volume expansion during hydrogenation, which in turn reduces PCT hysteresis and pulverization tendency [181], which results in a shorter cycle life [42]. Reports of V lowering capacity are also available [42].

6.2.2. Chromium

The addition of Cr in C14 MH alloys improves cycle stability [11,131,182,183,184,185] and charge retention [11,184,186] but decreases the HRD [11,186,187], capacity [131], and activation tendency [11]. Cr can suppress segregation of Ti, Zr, and V on the surface of MH alloys [188], retarding the oxidation of V by forming a V-based bcc solid solution secondary phase [131,189], and slowing down pulverization [190]. Retarding HRD by adding Cr was further attributed to poor bulk hydrogen diffusibility and surface exchange current [133]. Compared to Co, Cr promotes a dendritic grain structure that is beneficial for cycle stability [118]. Its capability of reducing PCT hysteresis also contributes to a longer cycle life [11].

6.2.3. Manganese

Partial replacement of Ni by Mn increases capacity [17,186], facilitating the formation process [186], but deteriorating the cycle life of the battery because of its poor oxidation resistance [186,191] and results in micro short-circuits [192]. A high Mn-content in an alloy reduces the cycle life and charge retention because of poor oxidation resistance in the KOH electrolyte [11]. A low Mn-content provides improves activation, capacity, and HRD [193]. Therefore, a careful balance between the content of Mn- and other B-elements is necessary to optimize battery performance [11,42]. In a separate report, Mn was found to increase the discharge capacity and exchange current density while hindering HRD and cycle stability [194]. Mn facilitates homogenizing the chemical composition of different constituent phases in a multi-phase alloy system [11].

6.2.4. Iron

In V-containing C14 alloys, the addition of Fe facilitates activation, increases the discharge capacity and surface reaction area, decreases HRD [131] and hydrogen diffusibility, and impairs low-temperature performance [195]. However, reports also suggest that Fe contributes to a low capacity [42] and higher cycle life [196,197]. In a V-free C14 alloy, the addition of Fe improves low-temperature performance, but hinders cycle life and charge retention [144]. The solubility of Fe in Zr7Ni10 and Zr9Ni11 phases is lower than that in TiNi phases, which explains the promotion of TiNi phase by Fe-addition [195].

6.2.5. Cobalt

Co promotes an equiaxial grain structure that improves surface reaction kinetics, activation, and capacity, but deteriorates cycle stability [196]. An optimal Co-content in a C14 MH alloy of 1.5 at % provides the best performance in terms of formation, cycle life, and charge retention, but exhibits worse specific power and low-temperature performance compared to other compositions [111]. Compared to other modifiers, such as Fe, Cu, Mo, and Al, Co-substituted C14 MH alloys show a relatively higher discharge capacity [120,198,199], good cycle performance [120,193,199], and poor HRD [152]. Reports on Co-substituted C14 MH alloys with increased plateau pressure [200], a reduced capacity [200], and a lower cycle life [42] are also available.

6.2.6. Nickel

Ni is the most efficient catalytic B-site element because of the formation of metallic clusters embedded in the surface oxide after activation [87,201,202]. The introduction of Ni greatly improves electrochemical behavior [203], HRD [11], low-temperature performance [11,202], surface exchange current [204], and cycle stability [186], but impedes charge retention [11].

6.2.7. Copper

In a typical C14 MH alloy, the addition of Cu, with is high degree of pulverization, facilitates activation processes and improves discharge capacity and low-temperature performance, but decreases HRD because of lower hydrogen diffusibility [205]. Cu has also been reported to impair cycle stability [206] and lower capacity [42].

6.2.8. Zinc

Zn has an extremely low melting point compared to its neighbors’ in the periodic table (Table 6) and is unable to remain in the C14 alloy at a melting point above 1350 °C. Therefore, ZnNi [207] and ZnCu [208] IMCs were used as raw materials to reduce Zn loss from evaporation. 1 at % Zn results in an increase in discharge capacities, a slight decrease in HRD, an easier activation process, and a satisfactory low-temperature performance [207].

6.2.9. Second Row Transition Metals (Mo)

Mo is the only element in the second row of transition metals that is used as a modifier in the C14 MH alloys, as it is accessible and not very toxic. According to our recent study, partial substitution of Co by Mo in a C14 MH alloy increases both the bulk diffusibility of hydrogen and surface catalytic ability, which leads to improved HRD and low-temperature performance [209]. Mo also improves charge retention and cycle stability, but yields a slightly lower capacity [209]. The cycle stability improvement of C14 MH alloy using Mo was also reported [42]. However, reports on the negative impact of Mo on the capacity, cycle life, and activation of C14 MH alloy are also available, presumably due to lack of Cr or Co in the composition [197,199]. Partially replacing Cr with Mo increases the gaseous phase H-storage capacity [210,211], ease of activation, and HRD [212].

6.2.10. Third Row Transition Metals (W, Pt)

W and Pt are the only two elements in the third row of the transition metals that are used because of concerns with availability and weight. W improves corrosion resistance and self-discharge of C14 MH alloys [213]. The addition of Pt in a C14 ZrCrNi alloy with an annealing treatment improved HRD and capacity because of the high catalytic activity of Pt for hydrogen electrosorption processes [214].

6.2.11. Group 13 Elements (B, Al)

B exhibits excellent solubility in V-free C14 MH alloys and contributes to a lower capacity, a high HRD, and improved superior low-temperature performance [144]. In V-containing alloys, B increased cycle stability [215] and bulk diffusion [216], however it also results in decreased capacity and HRD [216]. Reports on the positive contributions of B to HRD and low-temperature performance in V-containing C14 alloys are also available [217]. Ball milling C14 alloys with B show improved cycle stability at the cost of a lowered capacity [218].
Al is the most frequently used non-transition metal in Laves phase MH alloys. Al use has been shown to strongly correlate with a high capacity and a good HRD performance [219]. Al additives, together with Co, positively contribute to activation, charge retention, HRD, and low-temperature performances [136,220]. In the gaseous phase, Al was also shown to reduce PCT hysteresis, which in turn retards pulverization [200]. This also contributes to a lower flammability, which enhances safety in powder handling [221]. Even with the highest leaching out rate observed in Table 4, Al has been reported to improve the corrosion resistance of alloys, leading to better charge retention performance [164,213,222].

6.2.12. Group 14 Elements (C, Si, Ge, Sn)

In V-free C14 alloys, the addition of C promotes the formation of a ZrC secondary phase and improves charge retention, but also deteriorates low-temperature performance, cycle life, and HRD [144]. In a Ti-only C14 alloy, adding C promoted the formation of a TiC secondary phase, which facilitated the activation and decreased the gaseous phase H-storage capacity [223]. In one Zr-based C14 MH alloy, C improved cycle stability [17].
The addition of Si to C14 MH alloys improved the self-discharge [17], high-temperature discharge performances [17,224,225], low-temperature performance [226], and cycle stability [17,226] with trade-offs for lower capacity caused by an inert layer of SiO2 on the surface of the alloy [224,225]. Si-incorporated C15 MH alloys’ improved low-temperature performance is attributed to a layer of Ni2O3 that formed on the metal surface and can be detected by transmission electron microscopy (TEM, CM200/FEG, Philips, Amsterdam, The Netherlands) [227]. Si also contributes to a lower flammability that enhances safety in powder handling [221]. Both Si and Ge additives to ZrCr2 MH alloy reduce gaseous phase H-storage capacity [228].
Zr is widely used in nuclear power plants because of its stability from a low neutron scattering cross-section. The costly separation process from Hf (neutron absorber) makes pure Zr metal expensive [229]. Future cost reduction of Zr is expected as the demand of a Hf-containing Zr for battery applications (Hf impurities do not matter since Hf is also a hydride former) increases. Currently, a large amount of Zircaloy (a Sn-Zr alloy [230]) scrap is available from demolished nuclear power plants and the addition of Sn is essential for cost reduction in raw materials. According to our own study, a small amount of Sn (0.1 at %) can improve activation, HRD, charge retention, and low-temperature performances at the expense of capacity and cycle life loss [219,231]. Sn also promotes the formation of detrimental secondary phases. Thus, the content of Sn should be limited [145].

6.2.13. Group 16 Elements (O, S, Se)

The only report on the addition of O, S, and Se to C14 MH alloys compares gaseous phase characteristics and shows the same order of effectiveness (S > Se > O) in raising plateau pressure and PCT hysteresis, increasing storage capacity, and reducing the PCT slope factor [232].

6.3. Secondary Phase Promoter

The addition of elements with large atomic radii, but extremely low solubility in Ti-Zr based AB2 MH alloys, in the Laves phase will form secondary phases either in an element form or a Ni-containing alloy form. These secondary phases may play an important role in the electrochemical performance of the host alloy.

6.3.1. Group 1 Elements (Li, K)

Li has an extremely low melting point and very high vapor pressure at liquid temperatures for C14 MH alloys, therefore adding Li at the last stage and in the mold results in failure. However, Li-incorporated AB5 MH alloys with their lower melting temperature, were successfully prepared by AM [233], VIM [234], and a diffusion method [235]. Li did promote unidentified secondary phases, based on XRD analysis [235]. KB was added in a Ti2Ni based MH alloy as a source of K and showed improved cycle stability [215].

6.3.2. Group 2 Elements (Mg)

Solubility of Mg in the Laves phase is extremely low (0.l–0.3 at % [143]). In V-containing C14 alloys, it forms a cubic secondary phase, which facilitated the formation process but did not improve other electrochemical properties [143]. In V-free C14 alloys, the addition of Mg formed a Mg2Ni secondary phase and improved low-temperature performance and charge retention, but hampered cycle life and HRD [144]. Ball milling with Mg2Ni can also introduce Mg into AB2 MH alloys [236]. In recent years, Mg and La were introduced to AB2 MH alloys by either remelting [237] or MA [238] with an AB2/superlattice alloy mixture where superlattice alloys contain both La and Mg.

6.3.3. Rare Earth (RE) Metals

A great number of studies have focused on how to solve the slow activation of RE-incorporated C14MH alloys [67,165,184,239,240,241,242,243]. Low solubility of RE in Zr, Ti-based C14 IMC promotes a RE-Ni (AB) secondary phase and facilitates activation processes [244]. Properties of commonly used REs as modifiers in the AB2 MH alloy are summarized in Table 7. La, Ce, and Sm are the least expensive. In general, the ionic radius, ease of oxidation, and MH-bond strength become smaller when the atomic number increases. Previous studies in a comparison series of RE-doped C14 MH alloys [112,113,138,139,140,141] showed that the RE-Ni phase is beneficial for activation, but detrimental to HRD and low-temperature performance, and that a careful stoichiometric design is needed to balance the abundance of the RE-Ni and TiNi phases [113]. The incorporation of La provides the greatest low-temperature performance, but a contradictory microstructure (an increase in the detrimental LaNi phase and corresponding decrease in the beneficial TiNi phase). Further TEM studies indicated that the Ni-Cr alloy channeled and catalyzed by a single-crystal sheet contributes to improvements in the surface catalytic ability of La-incorporated alloys [95]. Gd remains as a metallic inclusion when melted with C14 MH alloys and improves low-temperature performance, but deteriorates HRD, cycle stability, and charge retention [144]. Instead of using RE, which are nearly insoluble in Laves phase alloys, MA was used and achieved similar effects of capacity and activation [245]. In addition to adding RE in elemental form, RE-containing AB5 [246,247] and A2B7 [248] can be used for similar results.

6.4. Summary of Modifier Studies

Unlike AB5, AB2 MH alloys are compatible with a remarkable number of elements. The degree of impact for commonly used elements on MH alloy properties are summarized in Table 8. Proper selection of elements can be based on the alloy requirements after checking each of the seven rows. Meanwhile, the pros and cons of each element can be easily evaluated in the corresponding column.

7. Stoichiometry

An IMC with a fixed stoichiometry comes with a large negative heat formation [45]. The different energy levels of anti-site and vacancy defects in a specific IMC may change its stoichiometry range [251,252,253]. If the energy for such defects is relatively low, a wide range of compositions (off-stoichiometry) are expected, among which AB2 Laves phase alloys make up the largest portion in IMC [21]. Compositions of a few IMCs based on Group 4 elements (Ti, Zr, and Hf) as A-site atoms are listed in Table 9 and plotted in Figure 15 as a function of RA/RB. IMCs with a C14 structure have a wider composition range (more likely to suffer from point defects) and the phase solubility of IMCs with a C15 structure becomes larger as the radii ratio increases. An AB2 alloy with a B/A ratio below 2.0 is a hypo-stoichiometric IMC. The reason that more hypo-stoichiometric IMCs tend to form as the radii ratio increases is that a relatively small B-atom more rapidly forms a double B in A-site (dumbbell model [254]) and further increases the B/A ratio. The characteristics of a few off-stoichiometric C14 MH alloys were previously compared [45,255,256] and important results are summarized in the next three sections.

7.1. Stoichiometric Alloy

The stoichiometric C14 MH alloys with a B/A ratio close to 2.0 have the highest electrochemical capacity and surface exchange current, and the smallest PCT hysteresis (least pulverization) [256] and is the most studied alloy stoichiometry in the field of battery applications.

7.2. Hypo-Stoichiometry

A C14 alloy with a B/A ratio below 2.0 is a hypo-stoichiometric IMC. The relatively low B/A ratio promotes the occurrence of AB phase (typically TiNi with a B2 structure) and improves activation behavior [256]. In a MS + annealing sample, the additional Ti (hypo-stoichiometry) increases both the capacity and cycle life of the electrode [64]. In a gaseous phase study of a TiCr based C14 alloy, a hypo-stoichiometry ratio (B/A of 1.8) gave the highest H-storage capacity [211].

7.3. Hyper-Stoichiometry

A hyper-stoichiometric C14 alloy has a B/A ratio higher than 2.0 and shows a high HRD [151,256], a high open-circuit voltage (from a higher PCT hydrogen equilibrium pressure) [256], and a flat PCT plateau [256]. The hyper-stoichiometric alloy also shows an improved cycle life, due to increased mechanical stability during cycling [185,258]. As x increases in a series of hyper-stoichiometric alloys ABx (x = 2–6), the bcc phase abundance increases, and results in improvements in capacity, kinetics [259], and cycle stability [260].

8. Discussions

The Ovonic Battery Company (Troy, MI, USA) focused on research about AB2 MH alloys for Ni/MH battery applications for more than three decades before being acquired by BASF (Ludwigshafen, Germany) in 2012. Throughout the years, we witnessed changing market demands and the corresponding reaction from the research communities. Before the successful debut of the commercialized Ni/MH battery in 1988, two main hurdles of the AB2 MH alloy were slow activation and poor cycle stability. While the former was addressed by fluorination and hot alkaline baths, the latter was improved substantially by composition modifications, mainly the introduction of Cr and consequent bcc secondary phase. The challenge to the first generation AB2-made Ni/MH battery was the self-discharge and was solved by the combination of V-free alloys and the use of the sulfonated separator. At that stage, AB2 MH alloys were successfully used in products made by Hitachi-Maxell (Tokyo, Japan), Gold-peak (Hong Kong, China), and General Motors (Detroit, MI, USA). With the cheap misch-metal (main raw material for the rival AB5 MH alloy) available from China, AB2 MH alloys started to phase out from the consumer market at the turn of the century. Later, the upset of RE prices in 2010 created opportunities for AB2 MH alloys. However, the bar to enter the market has not been raised in favor of AB2, mostly in the high-rate dischargeability requirement for HEV and power tools. The superlattice alloy used by FDK (Tokyo, Japan), Panasonic (Osaka, Japan), and Kawasaki Heavy Industry (Tokyo, Japan) became a strong competitor with a capacity between AB2 and AB5, but better high-rate performance. Mg, an indispensable element in the superlattice alloy, makes it more vulnerable to KOH electrolyte attack, but was mitigated using surfactant additives in the negative electrode paste [44]. The structure of the superlattice allows the removal of Mn and Co from the composition and improves the charge-retention characteristics tremendously [261]. At the current stage, AB2 has a hard time competing with AB5 in term of price and superlattice alloys in terms of performance.
However, new opportunities started to appear when the conventional Ni/MH battery based on the RE-based AB5 or A2B7 alloy lost the battle against the rival Li-ion technology. New applications require greater performance improvement in certain areas. For example, a solid-state battery with a thin solid separator [262] and ultra-high-power application with a very thin separator require a spherical MH alloy shape, which can be produced using GA techniques. Superlattice alloy with Mg inside cannot tolerate the Mg-vaporization because of the large surface area of the powder produced in the GA process, whereas GA with an associated annealing process already been successfully developed for AB2 MH alloy [62]. The battery/fuel cell combination requires a MH alloy operated at intermediate temperature range (200–250 °C) [263]. The other opportunity is in stationary applications that require tolerance in the environment of above 50 °C [3,4,264]. While the RE-containing AB5 and A2B7 MH alloys form an impeccable surface oxide in the high-temperature environment, the transition metal-based AB2 MH alloys leach out at a higher speed and are totally controllable by the composition re-adjustment. In the case of the new start-stop automobile application, a low-temperature cranking power is desperately needed [265]. There are a few elements contributing to the low-temperature performance of AB2 MH alloys through different mechanisms, for example, Y for surface area increase, La, Pd and Mo for surface catalytic ability improvement, and Fe for the increase of beneficial TiNi secondary phase. The pouch cell design (like commercially available Li-ion battery for cell phones) of Ni/MH battery operating under a flooded electrolyte configuration requires new MH alloys with a very low plateau pressure and a highly electrochemically catalytic surface [266,267]. The last example is the need for new high-capacity MH alloys that fully utilize the wide voltage window of the newly developed ionic liquid electrolyte [268]. The new chemical environment (electrolyte interface) and lifting of voltage constraint (from competition of hydrogen evolution) present new challenges (i.e., opportunities) for the development of new MH alloys. Although the function of each modifying element in specific areas has been studied and reported in the current work, combinations and the accompanying synergetic effects among these elements have not been reported. Therefore, a review like the current work only provides a guideline for future research. Readers are encouraged to use the results of this study to pursue further performance improvements in C14 Laves phase based MH alloys.

9. Conclusions

The main advantages of C14 Laves phase based metal hydride alloys are higher capacities and flexibilities in composition, stoichiometry, and constituent phases, which allow fine tailoring in the electrochemical performance to meet the demands of different applications. Decades of research in this area have already solved historical hurdles in C14-based alloys, such as slow activation, low cycle life, high self-discharge, and poor low-temperature performance. To face the new challenges from future applications, we have compiled comprehensive comparisons of preparation methods, alloy property requirements, the pros and cons of each constituting/modifying element, and choice of stoichiometry in the current study. Based on these previous works, new directions for additional improvement in the electrochemical performance should focus on the combination of modifier elements with different functions.

Acknowledgments

The authors would like to thank the following individuals from BASF-Ovonic making contributions to the ongoing research in AB2 MH alloys: Michael A. Fetcenko, Taihei Ouchi, Jean Nei, Diana F. Wong, Benjamin Reichman, Sherry Hu, John Koch, Suiling Chen, Cheryl Setterington, David Pawlik, Allen Chan, and Ryan J. Blankenship and former employees of Ovonics: Marvin Siskind, Su Cronogue, Jun Im, Joseph Tribu, Timothy Gizinski, David Smith, Xiaorong Tang, Crystal Yeh, Aereon Bisel, Anna Lewis, Lixin Wang, Tiejun Meng, Baoquan Huang, Feng Li, Melanie Reinhout, Nan Yu, Betty Cai, and Benjamin Chao for their technical assistance and valuable contributions. Kwo-Hsiung Young is obligated to his long-time partners in research: Ronald Tsang from Gold Peak, Koichi Morii from Daido Steel, Shigekazu Yasuoka from FDK Co., Leonid A. Bendersky from the National Institute of Standards and Technology, and Simon Ng from Wayne State University.

Author Contributions

Kwo-Hsiung Young prepared the main text and photographs. Shiuan Chang and Xinting Lin helped in the preparation of manuscript.

Conflicts of Interest

The authors declare no conflict of interest.

Abbreviations

The following abbreviations are used in this manuscript:
Ni/MHNickel/metal hydride
MHMetal hydride
H-storageHydrogen-strorage
VIMVacuum induction melting
AMArc melting
CCCentrifugal casting
MSMelt spinning
GAGas atomization
MAMechannical alloying
PSPlasma spray
SEMScanning electron microscope
bccBady-centered cubic
HRDHigh-rate dischargeability
M-Hmetal-hydrogen
RERare-earth elements
PCTPressure-concomposition-temperature
EVElectric vehicle
HEVHybrid electric vehicle
N/PNegative/Positive
HIAHydrogen-induced amorphization
IMCIntermettalic compound
TEMTransmission electron microscope

References

  1. Cai, X.; Young, K.; Chang, S. Reviews on the Chinese Patent regarding nickel/metal hydride battery. Batteries 2017, 3, 24. [Google Scholar] [CrossRef]
  2. Ogawa, K. Toyota to Start Local Production of NiMH Battery Cells in China by End of 2016. Available online: http://techon.nikkeibp.co.jp/atclen/news_en/15mk/030900433/ (accessed on 2 November 2016).
  3. Zelinsky, M.; Koch, J.; Fetcenko, M. Heat Tolerant NiMH Batteries for Stationary Power. Available online: www.battcon.com/PapersFinal2010/ZelinskyPaper2010Final_12.pdf (accessed on 28 March 2016).
  4. Zelinsky, M.; Koch, J. Batteries and Heat—A Recipe for Success? Available online: www.battcon.com/PapersFinal2013/16-Mike%20Zelinsky%20-%20Batteries%20and%20Heat.pdf (accessed on 28 March 2016).
  5. Teraoka, H. Development of Ni-MH ESS with Lifetime and Performance Estimation Technology. In Proceedings of the 34th International Battery Seminar & Exhibit, Fort Lauderdale, FL, USA, 20–23 March 2017. [Google Scholar]
  6. Teraoka, H. Ni-MH Stationary Energy Storage: Extreme Temperature & Long Life Developments. In Proceedings of the 33th International Battery Seminar & Exhibit, Fort Lauderdale, FL, USA, 21–24 March 2016. [Google Scholar]
  7. Teraoka, H. Development of Highly Durable and Long Life Ni-MH Batteries for Energy Storage Systems. In Proceedings of the 32th International Battery Seminar & Exhibit, Fort Lauderdale, FL, USA, 9–12 March 2015. [Google Scholar]
  8. Young, K.; Ouchi, T.; Nei, J.; Yasuoka, S. Fe-substitution for Ni in misch metal-based superlattice hydrogen absorbing alloys—Part 1. Structural, hydrogen storage, and electrochemical properties. Batteries 2016, 2, 34. [Google Scholar] [CrossRef]
  9. Kai, T.; Ishida, J.; Yasuoka, S.; Takeno, K. The Effect of Nickel-Metal Hydride Battery’s Characteristics with Structure of the Alloy. In Proceedings of the 54th Battery Symposium, Osaka, Japan, 7–9 October 2013; p. 210. [Google Scholar]
  10. Fetcenko, M.A.; Ovshinsky, S.A.; Young, K.; Reichman, B.; Fierro, C.; Koch, J.; Martin, F.; Mays, W.; Ouchi, T.; Sommers, B.; et al. High catalytic activity disordered VTiZrNiCrCoMnAlSn hydrogen storage alloys for nickel–metal hydride batteries. J. Alloys Compd. 2002, 330, 752–759. [Google Scholar] [CrossRef]
  11. Young, K.; Ouchi, T.; Koch, J.; Fetcenko, M.A. The role of Mn in C14 Laves phase multi-component alloys for NiMH battery application. J. Alloys Compd. 2009, 477, 749–758. [Google Scholar] [CrossRef]
  12. Young, K.; Yasuoka, S. Past, Present, and Future of Metal Hydride Alloys in Nickel-Metal Hydride Batteries. In Proceedings of the MH2014 Conference, Salford, UK, 20–25 July 2014. [Google Scholar]
  13. Chang, S.; Young, K.; Nei, J.; Fierro, C. Reviews on the U.S. Patents regarding nickel/metal hydride batteries. Batteries 2016, 2, 10. [Google Scholar] [CrossRef]
  14. Young, K.; Nei, J. The current status of hydrogen storage alloy development for electrochemical applications. Materials 2013, 6, 4574–4608. [Google Scholar] [CrossRef] [PubMed]
  15. Feng, F.; Geng, M.; Northwood, D.O. Electrochemical behaviour of intermetallic-based metal hydrides used in Ni/metal hydride (MH) batteries: A review. Int. J. Hydrogen Energy 2001, 26, 725–734. [Google Scholar] [CrossRef]
  16. Kleperis, J.; Wójcik, G.; Czerwinski, A.; Skowronski, J.; Kopxzyk, M.; Beltowska-Brzezinska, M. Electrochemical behavior of metal hydrides. J. Solid State Electrochem. 2001, 5, 229–249. [Google Scholar] [CrossRef]
  17. Han, S.; Zhao, M.; Wu, L.; Zheng, Y. Effect of additive elements on electrochemical properties of AB2-type Laves phase alloys. Chem. J. Chin. Univ. 2003, 24, 2256–2259. (In Chinese) [Google Scholar]
  18. Wang, J.; Yu, R.; Liu, Q. Effects of alloying side B on Ti-based AB2 hydrogen storage alloys. J. Harbin Inst. Technol. (New Ser.) 2004, 11, 485–492. [Google Scholar]
  19. Zhao, X.; Ma, L. Recent progress in hydrogen storage alloys for nickel/metal hydride secondary batteries. Int. J. Hydrogen Energy 2009, 34, 4788–4796. [Google Scholar] [CrossRef]
  20. Ouyang, L.; Huang, J.; Wang, H.; Liu, J.; Zhu, M. Progress of hydrogen storage alloys for Ni-MH rechargeable power batteries in electric vehicles: A review. Mater. Chem. Phys. 2017, 200, 164–178. [Google Scholar] [CrossRef]
  21. Stein, F.; Palm, M.; Sauthoff, G. Structure and stability of Laves phases. Part I. Critical assessment of factors controlling Laves phase stability. Intermetallics 2011, 12, 713–720. [Google Scholar] [CrossRef]
  22. Kumar, K.S.; Hazzledine, P.M. Polytypic transformations in Laves phases. Intermetallics 2004, 12, 763–770. [Google Scholar] [CrossRef]
  23. Chisholm, M.F.; Kumar, S.; Hazzledine, P. Dislocations in complex materials. Sciences 2005, 307, 701–703. [Google Scholar] [CrossRef] [PubMed]
  24. Baumann, W.; Leineweber, A.; Mittemeijer, E.J. The kinetics of a polytypic Laves phase transformation in TiCr2. Intermetallics 2011, 19, 526–535. [Google Scholar] [CrossRef]
  25. Scudino, S.; Donnadieu, P.; Surreddi, K.B.; Nikolowski, K.; Stoica, M.; Eckert, J. Microstructure and mechanical properties of Laves phase-reinforced Fe–Zr–Cr alloys. Intermetallics 2009, 17, 532. [Google Scholar] [CrossRef]
  26. Abraham, D.P.; Richardson, J.W., Jr.; McDeavitt, S.M. Laves intermetallics in stainless steel–zirconium alloys. Mater. Sci. Eng. A 1997, 239–240, 658–664. [Google Scholar] [CrossRef]
  27. Young, K.; Nei, J.; Wan, C.; Yartys, V. Comparison of C14- and C15-predominated AB2 metal hydride alloys for electrochemical applications. Batteries 2017, 3, 22. [Google Scholar] [CrossRef]
  28. Laves Crystal Structure of Laves Phase. Available online: http://www.geocities.jp/ohba_lab_ob_page/structure5.html (accessed on 26 April 2017).
  29. Young, K. Metal Hydride. In Elsevier Reference Module in Chemistry, Molecular Sciences and Chemical Engineering; Reedijk, J., Ed.; Elsevier: Waltham, MA, USA, 2013. [Google Scholar]
  30. Joubert, J.-M.; Latroche, M.; Percheron-Guégan, A.; Bouet, J. Improvement of the electrochemical activity of Zr–Ni–Cr Laves phase hydride electrodes by secondary phase precipitation. J. Alloys Compd. 1996, 240, 219–228. [Google Scholar] [CrossRef]
  31. Lee, H.-H.; Lee, K.-Y.; Lee, J.-Y. The hydrogenation characteristics of Ti-Zr-V-Mn-Ni C14 type Laves phase alloys for metal hydride electrodes. J. Alloys Compd. 1997, 253, 601–604. [Google Scholar] [CrossRef]
  32. Shu, K.Y.; Lei, Y.Q.; Yang, X.G.; Zhang, S.K.; Chen, L.S.; Lu, G.L.; Wang, Q.D. A comparative study on the electrochemical performance of rapidly solidified and conventionally cast hydride electrode alloy Zr(NiMnM)2.1. J. Alloys Compd. 1999, 290, 124–128. [Google Scholar] [CrossRef]
  33. Chen, L.; Wu, F.; Tong, M.; Chen, D.M.; Long, R.B.; Shang, Z.Q.; Liu, H.; Sun, W.S.; Yang, Y.; Wang, L.B.; et al. Advanced nanocrystalline Zr-based AB2 hydrogen storage electrode materials for NiMH EV batteries. J. Alloys Compd. 1999, 293, 508–520. [Google Scholar] [CrossRef]
  34. Zhu, Y.; Liu, Y.; Hua, F.; Li, L. Effect of rapid solidification on the structural and electrochemical properties of the Ti–V-based hydrogen storage electrode alloy. J. Alloys Compd. 2008, 463, 528–532. [Google Scholar] [CrossRef]
  35. Huang, S.S.; Chuang, H.J.; Chan, S.L.I. Effects of fluorination on the hydriding and electrochemical properties of a gas-atomized Zr-based hydrogen storage alloy. J. Alloys Compd. 2002, 330, 617–621. [Google Scholar] [CrossRef]
  36. Kim, J.H.; Lee, H.; Hwang, K.T.; Han, J.S. Hydriding behavior in Zr-based AB2 alloy by gas atomization process. Int. J. Hydrogen Energy 2009, 34, 9424–9430. [Google Scholar] [CrossRef]
  37. Jung, C.B.; Lee, K.S. Electrode characteristics of metal hydride electrodes prepared by mechanical alloying. J. Alloys Compd. 1997, 253, 605–608. [Google Scholar] [CrossRef]
  38. Qiu, S.J.; Chu, H.L.; Zhang, Y.; Sun, L.X.; Xu, F.; Cao, Z. The electrochemical performances of Ti–V-based hydrogen storage composite electrodes prepared by ball milling method. Int. J. Hydrogen Energy 2008, 33, 7471–7478. [Google Scholar] [CrossRef]
  39. Kazemipour, M.; Salimijazi, H.; Saidi, A.; Saatchi, A. Hydrogen storage properties of Ti0.72Zr0.28Mn1.6V0.4 alloy prepared by mechanical alloying and copper boat induction melting. Int. J. Hydrogen Energy 2014, 39, 12784–12788. [Google Scholar] [CrossRef]
  40. Kazemipour, M.; Salimijazi, H.; Saidi, A.; Saatchi, A.; Mostaghimi, J.; Pershin, L. The electrochemical hydrogen storage properties of Ti0.72Zr0.28Mn1.6V0.4 alloy synthesized by vacuum plasma spraying and vacuum copper boat induction melting: A comparative study. Int. J. Hydrogen Energy 2015, 40, 15569–15577. [Google Scholar] [CrossRef]
  41. Young, K.; Fetcenko, M.A.; Li, F.; Ouchi, T. Structural, thermodynamic, and electrochemical properties of TixZr1−x(VNiCrMnCoAl)2 C14 Laves phase alloys. J. Alloys Compd. 2008, 464, 238–247. [Google Scholar] [CrossRef]
  42. Izumi, Y.; Moriwaki, Y.; Yamashita, K.; Tokuhiro, T. Nickel-Metal Hydride Storage Battery and Alloy for Configuring Negative Electrode of the Same. U.S. Patent 5,962,156, 5 October 1999. [Google Scholar]
  43. Young, K.; Koch, J.; Ouchi, T.; Banik, A.; Fetcenko, M.A. Study of AB2 alloy electrodes for Ni/MH battery prepared by centrifugal casting and gas atomization. J. Alloys Compd. 2010, 496, 669–677. [Google Scholar] [CrossRef]
  44. Ouchi, T.; Young, K.; Moghe, D. Reviews on the Japanese Patent Applications regarding nickel/metal hydride batteries. Batteries 2016, 2, 21. [Google Scholar] [CrossRef]
  45. Young, K. Stoichiometry in inter-metallic compounds for hydrogen storage applications. In Stoichiometry and Materials Science—When Numbers Matter; Innocenti, A., Kamarulzaman, N., Eds.; InTech: Rijeka, Crotia, 2012. [Google Scholar]
  46. Humana, R.M.; Thomas, J.E.; Ruiz, F.; Real, S.G.; Castro, E.B.; Visintin, A. Electrochemical behavior of metal hydride electrode with different particle size. Int. J. Hydrogen Energy 2012, 37, 14966–14971. [Google Scholar] [CrossRef]
  47. Matsuoka, M.; Tamura, K. Effects of mechanical modification on electrochemical performance of Zr–Ti-based Laves-phase alloy electrode. J. Electrochem. Soc. 2007, 154, A119–A122. [Google Scholar] [CrossRef]
  48. Fetcenko, M.A.; Kaatz, T.; Sumner, S.P.; LaRocca, J. Hydride Reactor Apparatus for Hydrogen Comminution of Metal Hydride Hydrogen Storage Materials. U.S. Patent 4,893,756, 16 January 1990. [Google Scholar]
  49. Young, K.; Fetcenko, M.A. Method for Powder Formation of a Hydrogen Storage Alloy. U.S. Patent 6,120,936, 19 September 2000. [Google Scholar]
  50. Kim, D.M.; Lee, H.; Cho, K.; Lee, J.Y. Effect of Cu powder as an additive material on the inner pressure of a sealed-type Ni–MH rechargeable battery using a Zr-based alloy as an anode. J. Alloys Compd. 1999, 282, 261–267. [Google Scholar] [CrossRef]
  51. Tan, S.; Shen, Y.; Şahin, E.O.; Noréus, D.; Öztürk, T. Activation behavior of an AB2 type metal hydride alloy for NiMH batteries. Int. J. Hydrogen Energy 2016, 41, 9948–9953. [Google Scholar] [CrossRef]
  52. Liu, B.H.; Li, Z.P.; Okutsu, A.; Suda, S. A wet ball milling treatment of Zr-based AB2 alloys as negative electrode materials. J. Alloys Compd. 2000, 296, 148–151. [Google Scholar] [CrossRef]
  53. Great Powder Website. Available online: http://www.greatpowder.com/yingwen/ (accessed on 10 May 2017).
  54. Higuchi, E.; Li, Z.P.; Suda, S.; Nohara, S.; Inoue, H.; Iwakura, C. Structural and electrochemical characterization of fluorinated AB2-type Laves phase alloys obtained by different pulverization methods. J. Alloys Compd. 2002, 335, 241–245. [Google Scholar] [CrossRef]
  55. Hu, W.K.; Kim, D.M.; Jeon, S.W.; Lee, J.Y. Effect of annealing treatment on electrochemical properties of Mm-based hydrogen storage alloys for Ni/MH batteries. J. Alloys Compd. 1998, 270, 255–264. [Google Scholar] [CrossRef]
  56. Young, K.; Nei, J.; Ouchi, T.; Fetcenko, M.A. Phase abundances in AB2 metal hydride alloys and their correlations to various properties. J. Alloys Compd. 2011, 509, 2277–2284. [Google Scholar] [CrossRef]
  57. Young, K.; Ouchi, T.; Meng, T.; Wong, D.F. Studies on the synergetic effects in multi-phase metal hydride alloys. Batteries 2016, 2, 15. [Google Scholar] [CrossRef]
  58. Züttel, A.; Meli, F.; Chartouni, D.; Schlapbach, L.; Lichtenberg, F.; Friedrich, B. Properties of Zr(V0.25Ni0.75)2 metal hydride as active electrode material. J. Alloys Compd. 1996, 239, 175–282. [Google Scholar] [CrossRef]
  59. Zhang, Q.A.; Lei, Y.Q.; Yang, X.G.; Ren, K.; Wang, Q.D. Annealing treatment of AB2-type hydrogen storage alloys: I. crystal structures. J. Alloys Compd. 1999, 292, 236–240. [Google Scholar] [CrossRef]
  60. Zhang, Q.A.; Lei, Y.Q.; Yang, X.G.; Du, Y.L.; Wang, Q.D. Effects of annealing treatment on phase structures, hydrogen absorption–desorption characteristics and electrochemical properties of a V3TiNi0.56Hf0.24Mn0.15Cr0.1 alloy. J. Alloys Compd. 2000, 305, 125–129. [Google Scholar] [CrossRef]
  61. Young, K.; Ouchi, T.; Huang, B.; Chao, B.; Fetcenko, M.A.; Bendersky, L.A.; Wang, K.; Chiu, C. The correlation of C14/C15 phase abundance and electrochemical properties in the AB2 alloys. J. Alloys Compd. 2010, 506, 841–848. [Google Scholar] [CrossRef]
  62. Young, K.; Ouchi, T.; Banik, A.; Koch, J.; Fetcenko, M.A. Improvement in the electrochemical properties of gas atomized AB2 metal hydride alloys by hydrogen annealing. Int. J. Hydrogen Energy 2011, 36, 3547–3555. [Google Scholar] [CrossRef]
  63. Chuang, H.J.; Huang, S.S.; Ma, C.Y.; Chan, S.L.I. Effect of annealing heat treatment on an atomized AB2 hydrogen storage alloy. J. Alloys Compd. 1999, 285, 284–291. [Google Scholar] [CrossRef]
  64. Liu, H.; Li, R. Effect of variation of constituent on microstructure and electrochemical properties of AB2 hydrogen storage alloys. Foundry Technol. 2007, 29, 179–183. (In Chinese) [Google Scholar]
  65. Klein, B.; Simon, N.; Klyamkine, S.; Latroche, M.; Percheron-Guégan, A. Improvement of the thermodynamical and electrochemical properties of multicomponent Laves phase hydrides by thermal annealing. J. Alloys Compd. 1998, 280, 284–289. [Google Scholar] [CrossRef]
  66. Züttel, A.; Meli, F.; Schlapbach, L. Effects of pretreatment on the activation behavior of Zr(V0.25Ni0.75)2 metal hydride electrodes in alkaline solution. J. Alloys Compd. 1994, 209, 99–105. [Google Scholar] [CrossRef]
  67. Liu, F.J.; Kitayama, K.; Suda, S. La and Ce-incorporation effects on the surface properties of the fluorinated (Ti,Xr)(Mn,Cr,Ci)2 hydriding alloys. Vacuum 1996, 47, 903–906. [Google Scholar] [CrossRef]
  68. Liu, B.H.; Li, Z.P.; Higuchi, E.; Suda, S. Improvement of the electrochemical properties of Zr-based AB2 alloys by an advanced fluorination technique. J. Alloys Compd. 1999, 293, 702–706. [Google Scholar] [CrossRef]
  69. Li, Z.P.; Higuchi, E.; Liu, B.H.; Suda, S. Effects of fluorination temperature on surface structure and electrochemical properties of AB2 electrode alloys. Electrochim. Acta 2000, 45, 1773–1779. [Google Scholar] [CrossRef]
  70. Park, H.Y.; Cho, W.I.; Cho, B.W.; Lee, S.R.; Yun, K.S. Effect of fluorination on the lanthanum-doped AB2-type metal hydride electrodes. J. Power Sources 2001, 92, 149–156. [Google Scholar] [CrossRef]
  71. Li, Z.P.; Liu, B.H.; Hitaka, K.; Suda, S. Effects of surface structure of fluorinated AB2 alloys on their electrodes and battery performances. J. Alloys Compd. 2002, 330, 776–781. [Google Scholar] [CrossRef]
  72. Young, K.H.; Fetcenko, M.A.; Ovshinsky, S.R.; Ouchi, T.; Reichman, B.; Mays, W.C. Improved surface catalysis of Zr-based Laves phase alloys for NiMH batteries. In Hydrogen at Surface and Interfaces; Jerkiewicz, G., Feliu, J.M., Popov, B.N., Eds.; Electrochemical Society: Pennington, NJ, USA, 2000. [Google Scholar]
  73. Reichman, B.; Venkatesan, S.; Fetcenko, M.A.; Jeffries, K.; Stahl, S.; Bennett, C. Activated Rechargeable Hydrogen Storage Electrode and Method. U.S. Patent 4,716,088, 29 December 1987. [Google Scholar]
  74. Jung, J.H.; Liu, B.H.; Lee, J.Y. Activation behavior of Zr0.7Ti0.3Cr0.3Mn0.3V0.4Ni alloy electrode modified by the hot-charging treatment. J. Alloys Compd. 1998, 264, 306–310. [Google Scholar] [CrossRef]
  75. Liu, B.; Jung, J.; Lee, H.; Lee, K.; Lee, J. Improved electrochemical performance of AB2-type metal hydride electrode activated by the hot-charging process. J. Alloys Compd. 1996, 245, 132–141. [Google Scholar] [CrossRef]
  76. Cao, J.; Gao, X.; Lin, D.; Zhou, X.; Yuan, H.; Song, D.; Shen, P. Activation behavior of the Zr-based Laves phase alloy electrode. J. Power Sources 2011, 93, 141–144. [Google Scholar]
  77. Şahin, E.O. Development of Rare Earth-Free Negative Electrode Materials for NiMH Batteries. Proceeding of the 18th International Metallurgy & Materials Congress, Istanbul, Turkey, 29 September–1 October 2016; pp. 770–773. [Google Scholar]
  78. Jung, J.H.; Lee, H.H.; Kim, D.M.; Jang, K.J.; Lee, J.Y. Degradation behavior of Cu-coated Ti–Zr–V–Mn–Ni metal hydride electrodes. J. Alloys Compd. 1998, 266, 266–270. [Google Scholar] [CrossRef]
  79. Sun, D.; Latroche, M.; Percheron-Guégan, A. Activation behaviour of mechanically Ni-coated Zr-based laves phase hydride electrode. J. Alloys Compd. 1997, 257, 302–305. [Google Scholar] [CrossRef]
  80. Jurczyk, M.; Rajewski, W.; Majchrzycki, W.; Wojcik, G. Synthesis and electrochemical properties of high-energy ball-milled Laves phase (Zr,Ti)(V,Mn,Cr)2 alloys with nickel powder. J. Alloys Compd. 1998, 274, 299–302. [Google Scholar] [CrossRef]
  81. Lee, S.; Lee, H.; Yu, J.S.; Fateev, G.A.; Lee, J.Y. The activation characteristics of a Zr-based hydrogen storage alloy electrode surface-modified by ball-milling process. J. Alloys Compd. 1999, 292, 258–265. [Google Scholar] [CrossRef]
  82. Li, S.; Zhao, M.; Wang, Y.; Zhai, J. Structure and electrochemical property of ball-milled Ti0.26Zr0.07Mn0.1Ni0.33V0.24 alloy. Mater. Chem. Phys. 2009, 118, 51–56. [Google Scholar] [CrossRef]
  83. Chu, H.L.; Zhang, Y.; Sun, L.X.; Qiu, S.J.; Qi, Y.N.; Xu, F.; Yuan, H. Structure and electrochemical properties of composite electrodes synthesized by mechanical milling Ni-free TiMn2-based alloy with La-based alloy. J. Alloys Compd. 2007, 446–447, 614–619. [Google Scholar] [CrossRef]
  84. Li, P.; Wang, X.; Wu, J.; Zhao, W.; Li, R.; Ma, N. Present status on research of AB2-type Laves phase hydrogen storage electrode materials. Met. Funct. Mater. 2000, 7, 7–12. (In Chinese) [Google Scholar]
  85. Young, K. Electrochemical applications of metal hydride. In Compendium of Hydrogen Energy Volume 3: Hydrogen Energy Conversion; Barbir, F., Basile, A., Veziroglu, T.N., Eds.; Woodhead Publishing: Cambridge, UK, 2016. [Google Scholar]
  86. Hong, K. The development of hydrogen storage alloys and the progress of nickel hydride batteries. J. Alloys Compd. 2001, 321, 307–313. [Google Scholar] [CrossRef]
  87. Young, K.; Huang, B.; Regmi, R.K.; Lawes, G.; Liu, Y. Comparisons of metallic clusters imbedded in the surface oxide of AB2, AB5, and A2B7 alloys. J. Alloys Compd. 2010, 506, 831–840. [Google Scholar] [CrossRef]
  88. Young, K.; Ouchi, T.; Fetcenko, M.A. Pressure–composition–temperature hysteresis in C14 Laves phase alloys: Part 1. Simple ternary alloys. J. Alloys Compd. 2009, 480, 428–433. [Google Scholar] [CrossRef]
  89. Young, K.; Ouchi, T.; Mays, W.; Reichman, B.; Fetcenko, M.A. Pressure–composition–temperature hysteresis in C14 Laves phase alloys: Part 2. Applications in NiMH batteries. J. Alloys Compd. 2009, 480, 434–439. [Google Scholar] [CrossRef]
  90. Young, K.; Yasuoka, S. Capacity degradation mechanisms in nickel/metal hydride batteries. Batteries 2016, 2, 3. [Google Scholar] [CrossRef]
  91. Knosp, B.; Vallet, L.; Blanchard, P. Performance of an AB2 alloy in sealed Ni–MH batteries for electric vehicles: Quantification of corrosion rate and consequences on the battery performance. J. Alloys Compd. 1999, 293, 770–774. [Google Scholar] [CrossRef]
  92. Young, K.; Wong, D.F.; Yasuoka, S.; Ishida, J.; Nei, J.; Koch, J. Different failure modes for V-containing and V-free AB2 metal hydride alloys. J. Power Sources 2014, 251, 170–177. [Google Scholar] [CrossRef]
  93. Fetcenko, M.A.; Ovshinsky, S.R.; Reichman, B.; Young, K.; Fierro, C.; Koch, J.; Zallen, A.; Mays, W.; Ouchi, T. Recent advances in NiMH battery technology. J. Power Sources 2007, 165, 544–551. [Google Scholar] [CrossRef]
  94. Young, K.; Chao, B.; Liu, Y.; Nei, J. Microstructures of the oxides on the activated AB2 and AB5 metal hydride alloys surface. J. Alloys Compd. 2014, 606, 97–104. [Google Scholar] [CrossRef]
  95. Young, K.; Chao, B.; Pawlik, D.; Shen, H.T. Transmission electron microscope studies in the surface oxide on the La-containing AB2 metal hydride alloy. J. Alloys Compd. 2016, 672, 356–365. [Google Scholar] [CrossRef]
  96. Zhu, Y.; Pan, H.; Gao, M.; Liu, Y.; Li, R.; Lei, Y.; Wang, Q. Degradation mechanisms of Ti–V-based multiphase hydrogen storage alloy electrode. Int. J. Hydrogen Energy 2004, 29, 313–318. [Google Scholar] [CrossRef]
  97. Liu, B.H.; Li, Z.P.; Matsuyama, Y.; Kitani, R.; Suda, S. Corrosion and degradation behavior of Zr-based AB2 alloy electrodes during electrochemical cycling. J. Alloys Compd. 2000, 296, 201–208. [Google Scholar] [CrossRef]
  98. Chuang, H.J.; Chan, S.L.I. Study of the performance of Ti–Zr based hydrogen storage alloys. J. Power Sources 1999, 77, 159–163. [Google Scholar] [CrossRef]
  99. Aoki, K.; Yamamoto, T.; Masumoto, T. Hydrogen induced amorphization in RNi2 laves phases. Scr. Metall. 1987, 21, 27–31. [Google Scholar] [CrossRef]
  100. Aoki, K. Amorphous phase formation by hydrogen absorption. Mater. Sci. Eng. A 2001, 304–306, 45–53. [Google Scholar] [CrossRef]
  101. Aoki, K.; Masumoto, T. Hydrogen-induced amorphization of intermetallics. J. Alloys Compd. 1995, 231, 20–28. [Google Scholar] [CrossRef]
  102. Züttel, A.; Chartouni, D.; Nützenadel, C.; Gross, K.; Schlapbach, L. Bulk and surface properties of crystalline and amorphous Zr36(V0.33Ni0.66)64 alloy as active electrode material. J. Alloys Compd. 1998, 266, 321–326. [Google Scholar] [CrossRef]
  103. Hu, W.K.; Zhang, Y.S.; Song, D.Y.; Shen, P.W. Electrochemical hydrogen storage properties of amorphous and crystalline MI-Ni alloy films. Int. J. Hydrogen Energy 1996, 21, 651–656. [Google Scholar] [CrossRef]
  104. Zhao, X.; Ma, L.; Gou, Y.; Shen, X. Structure, morphology and hydrogen desorption characteristics of amorphous and crystalline Ti-Ni alloys. Mater. Sci. Eng. A 2009, 516, 50–53. [Google Scholar] [CrossRef]
  105. Yang, X.; Lei, Y.; Wang, C.; Zhu, G.; Zhang, W.; Wang, Q. Influence of amorphization on electrode performances of AB2 type hydrogen storage alloys. J. Alloys Compd. 1998, 265, 264–268. [Google Scholar] [CrossRef]
  106. Boettinger, W.J.; Newbury, D.E.; Wang, K.; Bendersky, L.A.; Chiu, C.; Kattner, U.R.; Young, K.; Chao, B. Examination of multiphase (Zr,Ti)(V,Cr,Mn,Ni)2 Ni-MH electrode alloys: Part I. Dendritic solidification structure. Metall. Mater. Trans. A 2010, 41, 2033–2047. [Google Scholar] [CrossRef]
  107. Bendersky, L.A.; Wang, K.; Boettinger, W.J.; Newbury, D.E.; Young, K.; Chao, B. Examination of multiphase (Zr,Ti)(V,Cr,Mn,Ni)2 Ni-MH electrode alloys: Part II. Solid-state transformation of the interdendritic B2 phase. Metall. Mater. Trans. A 2010, 41, 1891–1906. [Google Scholar] [CrossRef]
  108. Liu, Y.; Young, K. Microstructure investigation on metal hydride alloys by electron backscatter Diffraction Technique. Batteries 2016, 2, 26. [Google Scholar] [CrossRef]
  109. Bendersky, L.A.; Wang, K.; Levin, I.; Newbury, D.; Young, K.; Chao, B.; Creuziger, A. Ti12.5Zr21V10Cr8.5MnxCo1.5Ni46.5−x AB2-type metal hydride alloys for electrochemical storage application: Part 1. Structural characteristics. J. Power Sources 2012, 218, 474–486. [Google Scholar] [CrossRef]
  110. Tokunaga, T.; Motsumoto, S.; Ohtani, H.; Hasebe, M. Thermodynamic calculation of phase equilibria in the Nb-Ni-Ti-Zr quaternary system. Mater. Trans. 2007, 48, 89–96. [Google Scholar] [CrossRef]
  111. Young, K.; Ouchi, T.; Reichman, B.; Mays, W.; Regmi, R.; Lawes, G.; Fetcenko, M.A.; Wu, A. Optimization of Co-content in C14 Laves phase multi-component alloys for NiMH battery application. J. Alloys Compd. 2010, 489, 202–210. [Google Scholar] [CrossRef]
  112. Young, K.; Reichman, B.; Fetcenko, M.A. Electrochemical performance of AB2 metal hydride alloys measured at −40 °C. J. Alloys Compd. 2013, 580, S349–S352. [Google Scholar] [CrossRef]
  113. Young, K.; Wong, D.F.; Nei, J.; Reichman, B. Electrochemical properties of hypo-stoichiometric Y-doped AB2 metal hydride alloys at ultra-low temperature. J. Alloys Compd. 2015, 643, 17–27. [Google Scholar] [CrossRef]
  114. Zhang, Q.A.; Lei, Y.Q.; Wang, C.S.; Wang, F.S.; Wang, Q.D. Structure of the secondary phase and its effects on hydrogen-storage properties in a Ti0.7Zr0.2V0.1Ni alloy. J. Power Sources 1998, 75, 288–291. [Google Scholar] [CrossRef]
  115. Saldan, I.; Burtovyy, R.; Becker, H.W.; Ader, V.; Wöll, C. Ti–Ni alloys as MH electrodes in Ni–MH accumulators. Int. J. Hydrog. Energy 2008, 33, 7177–7184. [Google Scholar] [CrossRef]
  116. Nei, J.; Young, K. Gaseous phase and electrochemical hydrogen storage properties of Ti50Zr1Ni44X5 (X = Ni, Cr, Mn, Fe, Co, or Cu) for nickel metal hydride battery applications. Batteries 2016, 2, 24. [Google Scholar] [CrossRef]
  117. Emami, H.; Cuevas, F.; Latroche, M. Ti(Ni,Cu) pseudobinary compounds as efficient negative electrodes for Ni–MH batteries. J. Power Sources 2014, 265, 182–191. [Google Scholar] [CrossRef]
  118. Shu, K.Y.; Yang, X.G.; Zhang, S.K.; Lü, G.L.; Lei, Y.Q.; Wang, Q.D. Effect of Cr and Co additives on microstructure and electrochemical performance of Zr(NiVMn)2M0.1 alloys. J. Alloys Compd. 2000, 306, 122–126. [Google Scholar] [CrossRef]
  119. Young, K.; Chao, B.; Bendersky, L.A.; Wang, K. Ti12.5Zr21V10Cr8.5MnxCo1.5Ni46.5−x AB2-type metal hydride alloys for electrochemical storage application: Part 2. Hydrogen storage and electrochemical properties. J. Power Sources 2012, 218, 487–494. [Google Scholar] [CrossRef]
  120. Ji, S.; Li, S.; Sun, J. Effect of alloys with Mn, V on phase structures and electrochemical properties of Zr-Cr-Ni based AB2 hydrogen storage electrode alloys. Chin. J. Rare Met. 2004, 28, 657–661. (In Chinese) [Google Scholar]
  121. Nei, J.; Young, K.; Regmi, R.; Lawes, G.; Salley, S.O.; Ng, K.Y.S. Gaseous phase hydrogen storage and electrochemical properties of Zr8Ni21, Zr7Ni10, Zr9Ni11, and ZrNi metal hydride alloys. Int. J. Hydrogen Energy 2012, 37, 16042–16055. [Google Scholar] [CrossRef]
  122. Matsuyama, A.; Mizutani, H.; Kozuka, T.; Inoue, H. Effect of Ti substitution on electrochemical properties of ZrNi alloy electrode for use in nickel-metal hydride batteries. Int. J. Hydrogen Energy 2017. [Google Scholar] [CrossRef]
  123. Matsuyama, A.; Mizutani, H.; Kozuka, T.; Inoue, H. Crystal structure and hydrogen absorption-desorption properties of Zr1–xTixNi (0.05 ≤ x ≤ 0.5) alloys. J. Alloys Compd. 2017, 714, 467–475. [Google Scholar] [CrossRef]
  124. Ruiz, F.C.; Castro, E.B.; Real, S.G.; Peretti, H.A.; Visintin, A.; Triaca, W.E. Electrochemical characterization of AB2 alloys used for negative electrodes in Ni/MH batteries. Int. J. Hydrogen Energy 2008, 33, 3576–3580. [Google Scholar] [CrossRef]
  125. Ruiz, F.C.; Castro, E.B.; Peretti, H.A.; Visintin, A. Study of the different ZrxNiy phases of Zr-based AB2 materials. Int. J. Hydrogen Energy 2010, 35, 9879–9887. [Google Scholar] [CrossRef]
  126. Young, K.; Ouchi, T.; Liu, Y.; Reichman, B.; Mays, W.; Fetcenko, M.A. Structural and electrochemical properties of TixZr7−xNi10. J. Alloys Compd. 2009, 480, 521–528. [Google Scholar] [CrossRef]
  127. Young, K.; Ouchi, T.; Fetcenko, M.A.; Mays, W.; Reichman, B. Structural and electrochemical properties of Ti1.5Zr5.5VxNi10−x. Int. J. Hydrogen Energy 2009, 34, 8695–8706. [Google Scholar] [CrossRef]
  128. Nei, J.; Young, K.; Salley, S.O.; Ng, K.Y.S. Effects of annealing on Zr8Ni19X2 (X = Ni, Mg, Al, Sc, V, Mn, Co, Sn, La, and Hf): Hydrogen storage and electrochemical properties. Int. J. Hydrogen Energy 2012, 37, 8418–8427. [Google Scholar] [CrossRef]
  129. Young, M.; Chang, S.; Young, K.; Nei, J. Hydrogen storage properties of ZrVxNi3.5−x (x = 0.0–0.9) metal hydride alloys. J. Alloys Compd. 2013, 580, S171–S174. [Google Scholar] [CrossRef]
  130. Young, K.; Young, M.; Chang, S.; Huang, B. Synergetic effects in electrochemical properties of ZrVxNi4.5−x (x = 0.0, 0.1, 0.2, 0.3, 0.4, and 0.5) metal hydride alloys. J. Alloys Compd. 2013, 560, 33–41. [Google Scholar] [CrossRef]
  131. Zhu, Y.F.; Pan, H.G.; Wang, G.Y.; Gao, M.X.; Ma, J.X.; Chen, C.P.; Wang, Q.D. Phase structure, crystallography and electrochemical properties of Laves phase compounds Ti0.8Zr0.2V1.6Mn0.8−xMxNi0.6 (M = Fe, Al, Cr, Co). Int. J. Hydrogen Energy 2001, 26, 807–816. [Google Scholar] [CrossRef]
  132. Du, Y.L.; Yang, X.G.; Lei, Y.Q.; Zhang, M.S. Hydrogen storage properties of Zr0.8Ti0.2(Ni0.6Mn0.3−xV0.1+xCr0.05)2 (x = 0.0, 0.05, 0.15, 0.2) alloys. Int. J. Hydrogen Energy 2002, 27, 695–697. [Google Scholar] [CrossRef]
  133. Li, S.; Zhao, M.; Zhai, J.; Wang, F. Effect of substitution of chromium for nickel on structure and electrochemical characteristics of Ti0.26Zr0.07V0.24Mn0.1Ni0.33 multi-phase hydrogen storage alloy. Mater. Chem. Phys. 2009, 113, 96–102. [Google Scholar]
  134. Young, K.; Nei, J.; Wong, D.F.; Wang, L. Structural, hydrogen storage, and electrochemical properties of Laves phase-related body-centered-cubic solid solution metal hydride alloys. Int. J. Hydrogen Energy 2014, 39, 21489–21499. [Google Scholar] [CrossRef]
  135. Young, K.; Ng, K.Y.S.; Bendersky, L.A. A technical report of the robust affordable next generation energy storage system-BASF program. Batteries 2016, 2, 2. [Google Scholar] [CrossRef]
  136. Young, K.; Regmi, R.; Lawes, G.; Ouchi, T.; Reichman, B.; Fetcenko, M.A.; Wu, A. Effects of aluminum substitution in C14-rich multi-component alloys for NiMH battery application. J. Alloys Compd. 2010, 490, 282–292. [Google Scholar] [CrossRef]
  137. Iba, H.; Akiba, E. The relation between microstructure and hydrogen absorbing property in Laves phase-solid solution multiphase alloys. J. Alloys Compd. 1995, 231, 508–512. [Google Scholar] [CrossRef]
  138. Young, K.; Young, M.; Ouchi, T.; Reichman, B.; Fetcenko, M.A. Improvement in high-rate dischargeability, activation, and low-temperature performance in multi-phase AB2 alloys by partial substitution of Zr with Y. J. Power Sources 2012, 215, 279–287. [Google Scholar] [CrossRef]
  139. Young, K.; Wong, D.F.; Ouchi, T.; Huang, B.; Reichman, B. Effects of La-addition to the structure, hydrogen storage, and electrochemical properties of C14 metal hydride alloys. Electrochim. Acta 2015, 174, 815–825. [Google Scholar] [CrossRef]
  140. Young, K.; Ouchi, T.; Nei, J.; Moghe, D. The importance of rare-earth additions in Zr-based AB2 metal hydride alloys. Batteries 2016, 2, 25. [Google Scholar] [CrossRef]
  141. Wong, D.F.; Young, K.; Nei, J.; Wang, L.; Ng, K.Y.S. Effects of Nd-addition on the structural, hydrogen storage, and electrochemical properties of C14 metal hydride alloys. J. Alloys Compd. 2015, 647, 507–518. [Google Scholar] [CrossRef]
  142. Yoshida, M.; Ishibashi, H.; Susa, K.; Ogura, T.; Akiba, E. The multiphase effect on crystal structure, hydrogen absorbing properties and electrode performance of Sc-Zr based Laves phase alloys. J. Alloys Compd. 1995, 230, 100–108. [Google Scholar] [CrossRef]
  143. Chang, S.; Young, K.; Ouchi, T.; Meng, T.; Nei, J.; Wu, X. Studies on incorporation of Mg in Zr-based AB2 metal hydride alloys. Batteries 2016, 2, 11. [Google Scholar] [CrossRef]
  144. Young, K.; Ouchi, T.; Huang, B.; Fetcenko, M.A. Effects of B, Fe, Gd, Mg, and C on the structure, hydrogen storage, and electrochemical properties of vanadium-free AB2 metal hydride alloy. J. Alloys Compd. 2012, 511, 242–250. [Google Scholar] [CrossRef]
  145. Liu, H.; Li, R. Effect of Sn content on properties of AB2 hydrogen storage alloy. Foundry Technol. 2006, 27, 503–505. (In Chinese) [Google Scholar]
  146. Pottgen, R.; Dronskowski, R. Structure and properties of Zr2Ni2In and Zr2Ni2Sn. J. Solid State Chem. 1997, 128, 289–294. [Google Scholar] [CrossRef]
  147. Pearson, W.B. The Crystal Chemistry and Physics of Metals and Alloys; Wiley—Interscience: New York, NY, USA, 1972; p. 59. [Google Scholar]
  148. Nihon, K.G. Hi Kagaku Ryouronteki Kinzokukan Kagoubutsu; Maruzen: Tokyo, Japan, 1975; p. 296. (In Japanese) [Google Scholar]
  149. Yukawa, H.; Nakatsuka, K.; Morinaga, M. Design of hydrogen storage alloys in view of chemical bond between atoms. Sol. Energy Mater. Sol. Cells 2000, 62, 75–80. [Google Scholar] [CrossRef]
  150. Liu, S.; Sun, D. The current research and the development trend of hydrogen storage alloy. Rare Met. Cem. Carbides 2005, 33, 46–51. (In Chinese) [Google Scholar]
  151. Kim, D.M.; Jeon, S.W.; Lee, J.Y. A study of the development of a high capacity and high performance Zr–Ti–Mn–V–Ni hydrogen storage alloy for Ni–MH rechargeable batteries. J. Alloys Compd. 1998, 279, 209–214. [Google Scholar] [CrossRef]
  152. Kim, S.R.; Lee, J.Y.; Park, H.H. A study of the activation behaviour of Zr-Cr-Ni-La metal hydride electrodes in alkaline solution. J. Alloys Compd. 1994, 205, 225–229. [Google Scholar] [CrossRef]
  153. Shu, K.; Zhang, S.; Lei, Y.; Lü, G.; Wang, Q. Effect of Ti on the structure and electrochemical performance of Zr-based AB2 alloys for nickel-metal rechargeable batteries. J. Alloys Compd. 2003, 349, 237–241. [Google Scholar] [CrossRef]
  154. Lee, H.H.; Lee, K.Y.; Lee, J.Y. Degradation mechanism of Ti-Zr-V-Mn-Ni metal hydride electrodes. J. Alloys Compd. 1997, 260, 201–207. [Google Scholar] [CrossRef]
  155. Züttel, A.; Meli, F.; Schlapbach, L. Surface and bulk properties of the TiyZr1−y(VxNi1−x)2 alloy system as active electrode material in alkaline electrolyte. J. Alloys Compd. 1995, 231, 645–649. [Google Scholar] [CrossRef]
  156. Visintin, A.; Peretti, H.A.; Tori, C.A.; Triaca, W.E. Hydrogen absorption characteristics and electrochemical properties of Ti substituted Zr-based AB2 alloys. Int. J. Hydrogen Energy 2001, 26, 683–689. [Google Scholar] [CrossRef]
  157. Sun, J.C.; Li, S.; Ji, S.J. Phase composition and electrochemical performances of the Zr1−xTixCr0.4Mn0.2 V0.1Ni1.3 alloys with 0.1 ≤ x ≤ 0.3. J. Alloys Compd. 2005, 404, 687–690. [Google Scholar] [CrossRef]
  158. Zhu, Y.F.; Pan, H.G.; Gao, M.X.; Ma, J.X.; Li, S.Q.; Wang, Q.D. The effect of Zr substitution for Ti on the microstructures and electrochemical properties of electrode alloys Ti1−xZrxV1.6Mn0.32Cr0.48Ni0.6. Int. J. Hydrogen Energy 2002, 27, 287–293. [Google Scholar] [CrossRef]
  159. Hariprakash, B.; Martha, S.K.; Shukla, A.K. Effect of copper additive on Zr0.9Ti0.1V0.2Mn0.6Cr0.05Co0.05Ni1.2 alloy anode for nickel-metal hydride batteries. J. Appl. Electrochem. 2003, 33, 497–504. [Google Scholar] [CrossRef]
  160. Huot, J.; Akiba, E.; Ogura, T.; Ishido, Y. Crystal structure, phase abundance and electrode performance of Laves phase compounds (Zr, A)V0.5Ni1.1Mn0.2Fe0.2 (A≡Ti, Nb or Hf). J. Alloys Compd. 1995, 218, 101–109. [Google Scholar] [CrossRef]
  161. Huot, J.; Akiba, E.; Ishido, Y. Crystal structure of multiphase alloys (Zr,Ti)(Mn,V)2. J. Alloys Compd. 1995, 231, 85–89. [Google Scholar] [CrossRef]
  162. Nei, J.; Young, K.; Salley, S.O.; Ng, K.Y.S. Determination of C14/C15 phase abundance in Laves phase alloys. Mater. Chem. Phys. 2012, 136, 520–527. [Google Scholar] [CrossRef]
  163. Kandavel, M.; Bhat, V.V.; Rougier, A.; Aymard, L.; Nazri, G.A.; Tarascon, J.M. Improvement of hydrogen storage properties of the AB2 Laves phase alloys for automotive application. Int. J. Hydrogen Energy 2008, 33, 3754–3761. [Google Scholar] [CrossRef]
  164. Wakao, S.; Sawa, H.; Furukawa, J. Effects of partial substitution and anodic oxidation treatment of Zr–V–Ni alloys on electrochemical properties. J. Less Common Met. 1991, 172, 1219–1226. [Google Scholar] [CrossRef]
  165. Kim, S.; Lee, J. Activation behaviour of ZrCrNiM0.05 metal hydride electrode (M = La, Mm (misch metal), Nd). J. Alloys Compd. 1992, 185, L1–L4. [Google Scholar] [CrossRef]
  166. Rönnebro, E.; Noréus, D.; Sakai, T.; Tsukahara, M. Structural studies of a new Laves phase alloy (Hf,Ti)(Ni,V)2 and its very stable hydride. J. Alloys Compd. 1995, 231, 90–94. [Google Scholar] [CrossRef]
  167. Huot, J.; Akiba, E.; Orura, O.; Ishido, Y. Crystal structure of electrode materials (Zr,A)V0.5Ni1.1Mn0.2Fe0.2 (A=Ti, Nb and Hf) for Ni-hydrogen rechargeable batteries. Trans. Mater. Res. Soc. Jpn. 1994, 18B, 1197–1200. [Google Scholar]
  168. Zhou, O.; Yao, Q.; Sun, X.; Gu, Q.; Sun, J. Lattice-substitution of alloying elements and its influences on mechanical properties of ZrCr2 Laves phase. Chin. J. Nonferr. Met. 2006, 16, 1603–1607. (In Chinese) [Google Scholar]
  169. Santos, A.R.; Ambrosio, R.C.; Ticianelli, E.A. Electrochemical and structural studies on nonstoichiometric AB2-type metal hydride alloys. Int. J. Hydrogen Energy 2004, 29, 1253–1261. [Google Scholar]
  170. Young, K.; Ouchi, T.; Nei, J.; Chang, S. Increase in the Surface Catalytic Ability by Addition of Palladium in C14 Metal Hydride Alloy. Batteries 2017, 3, 26. [Google Scholar] [CrossRef]
  171. Yang, X.G.; Zhang, W.K.; Lei, Y.Q.; Wang, Q.D. Electrochemical properties of Zr-V-Ni system hydrogen storage alloys. J. Electrochem. Soc. 1999, 146, 1245–1250. [Google Scholar] [CrossRef]
  172. Ovshinsky, S.R.; Young, R. High Power Nickel-Metal Hydride Batteries and High Power Alloys/Electrodes for Use Therein. U.S. Patent 6,413,670 B1, 2 July 2002. [Google Scholar]
  173. Yoshida, M.; Akiba, E. Hydrogen absorbing properties of ScM2 Laves phase alloys (M = Fe, Co and Ni). J. Alloys Compd. 1995, 226, 75–80. [Google Scholar] [CrossRef]
  174. Yoshida, M.; Ishibashi, H.; Susa, K.; Ogura, T.; Akiba, E. Crystal structure, hydrogen absorbing properties and electrode performances of Sc-based Laves phase alloys. J. Alloys Compd. 1995, 226, 161–165. [Google Scholar] [CrossRef]
  175. Li, K.; Luo, Y.; Wang, W.; Qiu, J.; Kang, L. Effects of scandium on hydrogen storage and electrochemical properties of AB2-type Zr1−xScxMn0.6V0.2Ni1.2Co0.1 (x = 0~1) alloys. J. Chin. Rare Earth Soc. 2013, 31, 442–449. (In Chinese) [Google Scholar]
  176. Liu, X.J.; Yang, S.Y.; Huang, Y.X.; Zhang, J.B.; Wang, C.P. Experimental investigation of isothermal sections (100, 1200 °C) in the Ni-Ti-Zr system. J. Ph. Equilib. Diffus. 2015, 36, 414–421. [Google Scholar] [CrossRef]
  177. Young, K.; Fetcenko, M.A.; Li, F.; Ouchi, T.; Koch, J. Effect of vanadium substitution in C14 Laves phase alloys for NiMH battery application. J. Alloys Compd. 2009, 468, 482–492. [Google Scholar] [CrossRef]
  178. Young, K.; Ouchi, T.; Koch, J.; Fetcenko, M.A. Compositional optimization of vanadium-free hypo-stoichiometric AB2 metal hydride alloy for Ni/MH battery application. J. Alloys Compd. 2012, 510, 97–106. [Google Scholar] [CrossRef]
  179. Wang, J.; Yu, R.; Liu, Q. Relation of element substitution to discharge capacity and activation of Ti-Zr based AB2-type hydrogen storage electrode alloys. Mater. Sci. Technol. 2005, 13, 166–170. (In Chinese) [Google Scholar]
  180. Yang, H.W.; Wang, Y.Y.; Wan, C.C. Studies of electrochemical properties of Ti0.35Zr0.65NixV2−xyMny alloys with C14 Laves phases for nickel/metal hydride batteries. J. Electrochem. Soc. 1996, 143, 429–435. [Google Scholar] [CrossRef]
  181. Hagström, M.T.; Klyamkin, S.N.; Lund, P.D. Effect of substitution on hysteresis in some high-pressure AB2 and AB5 metal hydrides. J. Alloys Compd. 1999, 293, 67–73. [Google Scholar] [CrossRef]
  182. Lee, S.F.; Wang, Y.Y.; Wan, C.C. Effect of adding chromium to Ti-Zr-Ni-V-Mn alloy on its cycle life as an Ni/metal-hydride battery material. J. Power Sources 1997, 66, 165–168. [Google Scholar] [CrossRef]
  183. Lee, H.; Lee, S.; Lee, J. Activation characteristics of multiphase Zr-based hydrogen storage alloys for Ni/MH rechargeable batteries. J. Electrochem. Soc. 1999, 146, 3666–3671. [Google Scholar] [CrossRef]
  184. Park, H.Y.; Chang, I.; Cho, W.I.; Cho, B.W.; Jang, H.; Lee, S.R.; Yun, K.S. Electrode characteristics of the Cr and La doped AB2-type hydrogen storage alloys. Int. J. Hydrogen Energy 2001, 26, 949–955. [Google Scholar] [CrossRef]
  185. Liu, B.H.; Li, Z.P.; Kitani, R.; Suda, S. Improvement of electrochemical cyclic durability of Zr-based AB2 alloy electrodes. J. Alloys Compd. 2002, 330, 825–830. [Google Scholar] [CrossRef]
  186. Young, K.; Ouchi, T.; Fetcenko, M.A. Roles of Ni, Cr, Mn, Sn, Co, and Al in C14 Laves phase alloys for NiMH battery application. J. Alloys Compd. 2009, 476, 774–781. [Google Scholar] [CrossRef]
  187. Peretti, H.A.; Visintin, A.; Mogni, L.V.; Corso, H.L.; Gamboa, J.A.; Serafini, D.; Triaca, W.E. Hydrogen absorption behavior of multicomponent zirconium based AB2 alloys with different chromium–vanadium ratio. J. Alloys Compd. 2003, 354, 181–186. [Google Scholar] [CrossRef]
  188. Wang, G.Y.; Xu, Y.H.; Pan, H.G.; Wang, Q.D. Effect of substitution of chromium for manganese on structure discharge characteristics of Ti-Zr-V-Mn-Ni-type multi-phase hydrogen storage electrode alloys. Int. J. Hydrogen Energy 2003, 28, 499–508. [Google Scholar] [CrossRef]
  189. Pan, H.; Li, R.; Gao, M.; Liu, Y.; Wang, Q. Effects of Cr on the structural and electrochemical properties of TiV-based two-phase hydrogen storage alloys. J. Alloys Compd. 2005, 404, 669–674. [Google Scholar] [CrossRef]
  190. Yu, J.; Lee, S.; Cho, K.; Lee, J. The cycle life of Ti0.8Zr0.2V0.5Mn0.5–xCrxNi0.8 (x = 0 to 0.5) alloys for metal hydride electrodes of Ni-metal hydride rechargeable battery. J. Electrochem. Soc. 2000, 147, 2013–2017. [Google Scholar] [CrossRef]
  191. Xu, Y.H.; Chen, C.P.; Wang, X.L.; Lei, Y.Q.; Wang, Q.D. The cycle life and surface properties of Ti-based AB2 metal hydride electrodes. J. Alloys Compd. 2002, 337, 214–220. [Google Scholar] [CrossRef]
  192. Shinyama, K.; Magari, Y.; Akita, H.; Kumagae, K.; Nakamura, H.; Matsuta, S.; Nohma, T.; Takee, M.; Ishiwa, K. Investigation into the deterioration in storage characteristics of nickel-metal hydride batteries during cycling. J. Power Sources 2005, 143, 265–269. [Google Scholar] [CrossRef]
  193. Chen, J.; Dou, S.X.; Liu, H.K. Hydrogen desorption and electrode properties of Zr0.8Ti0.2(V0.3Ni0.6M0.1)2. J. Alloys Compd. 1997, 256, 40–44. [Google Scholar] [CrossRef]
  194. Chai, Y.J.; Zhao, M.S.; Wang, N. Crystal structural and electrochemical properties of Ti0.17Zr0.08V0.35Cr0.10Ni0.30−xMnx (x = 0–0.12) alloys. Mater. Sci. Eng. B 2008, 147, 47–51. [Google Scholar] [CrossRef]
  195. Young, K.; Ouchi, T.; Huang, B.; Reichman, B.; Fetcenko, M.A. The structure, hydrogen storage, and electrochemical properties of Fe-doped C14-predominating AB2 metal hydride alloys. Int. J. Hydrogen Energy 2011, 36, 12296–12304. [Google Scholar] [CrossRef]
  196. Song, M.Y.; Ahn, D.; Kwon, I.; Lee, R.; Rim, H. Development of AB2-type Zr–Ti–Mn–V–Ni–Fe hydride electrodes for Ni–MH secondary batteries. J. Alloys Compd. 2000, 298, 254–260. [Google Scholar] [CrossRef]
  197. Song, M.Y.; Kown, I.H.; Ahh, D.S.; Sohn, M.S. Improvement in the electrochemical properties of ZrMn2 hydrides by substitution of elements. Met. Mater. Int. 2001, 7, 257–263. [Google Scholar] [CrossRef]
  198. Kim, S.R.; Lee, J.Y. Electrode characteristics of C14-type Zr-based laves phase alloys. J. Alloys Compd. 1994, 210, 109–113. [Google Scholar] [CrossRef]
  199. Song, M.Y.; Ahn, D.; Kwon, I.H.; Chough, S.H. Development of AB2-type Zr-Ti-Mn-V-Ni-M hydride electrode for Ni/MH secondary battery. J. Electrochem. Soc. 2001, 148, A1041–A1044. [Google Scholar] [CrossRef]
  200. Honda, N.; Furukawa, N.; Fujitani, S.; Yonezu, I. Hydrogen Absorbing Modified ZrMn2-Type Alloys. U.S. Patent 4,913,879, 3 April 1990. [Google Scholar]
  201. Ovshinsky, S.R.; Fetcenko, M.A.; Ross, J. A nickel metal hydride battery for electric vehicles. Science 1993, 260, 176–181. [Google Scholar] [CrossRef] [PubMed]
  202. Kim, S.R.; Lee, K.Y.; Lee, J.Y. Improved low-temperature dischargeability of C14-type Zr–Cr–Ni Laves phase alloy. J. Alloys Compd. 1995, 223, 22–27. [Google Scholar] [CrossRef]
  203. Kwon, I.; Park, H.; Song, M. Electrochemical properties of ZrMnNi1+x hydrogen-storage alloys. Int. J. Hydrogen Energy 2002, 27, 171–176. [Google Scholar] [CrossRef]
  204. Lee, H.H.; Lee, K.Y.; Lee, J.Y. The Ti-based metal hydride electrode for NiMH rechargeable batteries. J. Alloys Compd. 1996, 239, 63–70. [Google Scholar] [CrossRef]
  205. Young, K.; Ouchi, T.; Huang, B.; Reichman, B.; Fetcenko, M.A. Studies of copper as a modifier in C14-predominant AB2 metal hydride alloys. J. Power Sources 2012, 204, 205–212. [Google Scholar] [CrossRef]
  206. Yamamura, Y.; Seri, H.; Tsuji, Y.; Owada, N.; Iwaki, T. Hydrogen Storage Alloy and Electrode Therefrom. U.S. Patent 5,532,076, 2 July 1996. [Google Scholar]
  207. Young, K.; Ouchi, T.; Lin, X.; Reichman, B. Effects of Zn-addition to C14 metal hydride alloys and comparisons to Si, Fe, Cu, Y, and Mo-additives. J. Alloys Compd. 2016, 655, 50–59. [Google Scholar] [CrossRef]
  208. Wang, Y.; Zhao, D.; Yuan, H.; Wang, G.; Zhou, Z.; Song, D.; Zhang, Y. Preparation and electrochemical properties of MI(NiCuAlZn)5 hydrogen storage alloys. Acta Sci. Bat. Univ. Nankaiensis 2000, 33, 120–123. (In Chinese) [Google Scholar]
  209. Young, K.; Ouchi, T.; Huang, B.; Reichman, B.; Fetcenko, M.A. Effect of molybdenum content on structural, gaseous storage, and electrochemical properties of C14-predominant AB2 metal hydride alloys. J. Power Sources 2011, 196, 8815–8821. [Google Scholar] [CrossRef]
  210. Au, M.; Pourarian, F.; Sankar, S.G.; Wallace, W.E.; Zhang, L. TiMn2-bases alloys as high hydrogen materials. Mater. Sci. Eng. B 1995, 33, 53–57. [Google Scholar] [CrossRef]
  211. Huang, T.; Wu, Z.; Xia, B.; Xu, N. Influence of stoichiometry and alloying elements on the crystallography and hydrogen sorption properties of TiCr based alloys. Mater. Sci. Eng. A 2005, 397, 284–287. [Google Scholar]
  212. Erika, T.; Ricardo, F.; Fabricio, R.; Fernando, Z.; Verónica, D. Electrochemical and metallurgical characterization of ZrCr1xNiMox AB2 metal hydride alloys. J. Alloys Compd. 2015, 649, 267–274. [Google Scholar] [CrossRef]
  213. Doi, H.; Yabuki, R. Hydrogen Absorbing Ni, Zr-Based Alloy and Rechargeable Alkaline Battery. U.S. Patent 4,898,794, 6 February 1990. [Google Scholar]
  214. Ruiz, F.C.; Peretti, H.A.; Visintin, A.; Triaca, W.E. A study on ZrCrNiPtx alloys as negative electrode components for NiMH batteries. Int. J. Hydrogen Energy 2011, 36, 901–906. [Google Scholar] [CrossRef]
  215. Luan, B.; Cui, N.; Zhao, H.J.; Liu, H.K.; Dou, S.X. Effects of potassium-boron addition on the performance of titanium based hydrogen storage alloy electrodes. Int. J. Hydrogen Energy 1996, 21, 373–379. [Google Scholar] [CrossRef]
  216. Reddy, A.L.M.; Ramaprabhu, S. Hydrogen diffusion studied in Zr-based Laves phase AB2 alloys. J. Alloys Compd. 2008, 460, 268–271. [Google Scholar] [CrossRef]
  217. Reddy, A.L.M.; Ramaprabhu, S. Structural and hydrogen absorption kinetics studies of polymer dispersed and boron added Zr-based AB2 alloy. Int. J. Hydrogen Energy 2006, 31, 867–876. [Google Scholar]
  218. Li, S.; Wen, B.; Li, X. Structure and electrochemical property of ball-milled Ti0.26Zr0.07Mn0.1Ni0.33V0.24 alloy with 3 mass% B. J. Alloys Compd. 2016, 654, 580–585. [Google Scholar] [CrossRef]
  219. Young, K.; Fetcenko, M.A.; Koch, J.; Morii, K.; Shimizu, T. Studies of Sn, Co, Al, and Fe additives in C14/C15 Laves alloys for NiMH battery application by orthogonal arrays. J. Alloys Compd. 2009, 486, 559–569. [Google Scholar] [CrossRef]
  220. Fetcenko, M.A.; Young, K.; Ovshinky, S.R.; Reichman, B.; Koch, J.; Mays, W. Modified Electrochemical Hydrogen Storage Alloy Having Increased Capacity, Rate Capability and Catalytic Activity. U.S. Patent 6,270,719, 7 August 2001. [Google Scholar]
  221. Gamo, T.; Moriwaki, Y.; Iwaki, T. Alloy for Hydrogen Storage Electrodes. U.S. Patent 4,946,646, 7 August 1990. [Google Scholar]
  222. Doi, H.; Yabuki, R. Hydrogen Absorbing Ni-Based Alloy and Rechargeable Alkaline Battery. U.S. Patent 4,983,474, 9 January 1991. [Google Scholar]
  223. Yu, X.B.; Wu, Z.; Huang, T.Z.; Chen, J.Z.; Xia, B.J.; Xu, N.X. Effect of carbon addition on activation and hydrogen sorption characteristics of TiMn1.25Cr0.25 alloy. Mater. Chem. Phys. 2004, 83, 273–277. [Google Scholar] [CrossRef]
  224. Young, K.; Ouchi, T.; Huang, B.; Reichman, B.; Blankenship, R. Improvement in −40 °C electrochemical properties of AB2 metal hydride alloy by silicon incorporation. J. Alloys Compd. 2013, 575, 65–72. [Google Scholar] [CrossRef]
  225. Han, S.; Zhoa, M.; Liu, B. Microstructure and high-temperature electrochemical characteristics of Zr0.9Ti0.1Ni1.0Mn0.7V0.3Six (x = 0.05, 0.10, 0.15, 0.20) alloy. Mater. Chem. Phys. 2005, 89, 221–227. [Google Scholar] [CrossRef]
  226. Li, S.; Liu, Y.; Zhu, J. Effect of Si-element on electrochemical properties of Ti-based hydrogen storage alloys. Titan. Ind. Prog. 2007, 24, 10–22. (In Chinese) [Google Scholar]
  227. Young, K.; Chao, B.; Nei, J. Microstructures of the activated Si-containing AB2 metal hydride alloy surface by transmission electron microscope. Batteries 2016, 2, 4. [Google Scholar] [CrossRef]
  228. Drašner, A.; Blaẑina, Ẑ. The influence of Si and Ge on the hydrogen sorption properties of the intermetallic compound ZrCr2. J. Alloys Compd. 1993, 199, 101–104. [Google Scholar]
  229. Xu, L.; Xiao, Y.; Sandwijk, A.; Xu, Q.; Yang, Y. Separation of zirconium and hafnium: A review. In Energy Materials 2014; Springer: Heidelberg, Germany, 2014; p. 451. [Google Scholar]
  230. Yamanaka, S.; Higuchi, K.; Miyake, M. Hydrogen solubility in zirconium alloys. J. Alloys Compd. 1995, 231, 503–507. [Google Scholar] [CrossRef]
  231. Young, K.; Fetcenko, M.A.; Ouchi, T.; Li, F.; Koch, J. Effect of Sn-substitution in C14 Laves phase alloys for NiMH battery application. J. Alloys Compd. 2009, 469, 406–416. [Google Scholar] [CrossRef]
  232. Morita, Y.; Gamo, T.; Kuranaka, S. Effects of nonmetal addition on hydriding properties for Ti–Mn Laves phase alloys. J. Alloys Compd. 1997, 253, 29–33. [Google Scholar] [CrossRef]
  233. Giza, K.; Isasieczko, W.; Pavlyuk, V.V.; Bala, H.; Drulis, H.; Adamczyk, L. Hydrogen absorption and corrosion resistance of LaNi4.8Al0.2 and LaNi4.8Al0.1Li0.1 alloy. J. Alloys Compd. 2007, 429, 352–356. [Google Scholar] [CrossRef]
  234. Wei, X.; Tang, R.; Liu, Y.; Zhang, P.; Yu, G.; Zhu, J. Effect of small amounts of Li on microstructures and electrochemical properties of non-stoichiometric low-Co AB5-type alloys. Int. J. Hydrogen Energy 2006, 31, 1365–1371. [Google Scholar] [CrossRef]
  235. Wang, L.; Yuan, H.; Yang, H.; Zhou, K.; Song, D.; Zhang, Y. Study of the multi-composition AB2 alloys including Li, made by the diffusion method, and their electrodes. J. Alloys Compd. 2000, 302, 65–69. [Google Scholar] [CrossRef]
  236. Cracco, D.; Percheron-Guégan, A. Morphology and hydrogen absorption properties of an AB2 type alloy ball milled with Mg2Ni. J. Alloys Compd. 1998, 268, 248–255. [Google Scholar] [CrossRef]
  237. Wang, Y.; Zhao, M. Electrochemical hydrogen storage characteristics of Ti0.10Zr0.15V0.35Cr0.10Ni0.30−10% LaNi3 composite and its synergetic effect. Trans. Nonferr. Met. Soc. China 2012, 22, 2000. (In Chinese) [Google Scholar] [CrossRef]
  238. Chu, H.; Zhang, Y.; Sun, L.; Qiu, S.; Xu, F.; Yuan, H.; Wang, Q.; Dong, C. Structure, morphology and hydrogen storage properties of composites prepared by ball milling Ti0.9Zr0.2Mn1.5Cr0.3V0.3 with La–Mg-based alloy. Int. J. Hydrogen Energy 2007, 32, 3363–3369. [Google Scholar] [CrossRef]
  239. Liu, F.J.; Sandrock, G.; Suda, S. Surface and metallographic microstructure of the La-added AB2 compound (Ti, Zr)(Mn, Cr, Ni)2. J. Alloys Compd. 1995, 231, 392–396. [Google Scholar] [CrossRef]
  240. Sun, D.; Latroche, M.; Percheron-Guégan, A. Effects of lanthanum or cerium on the equilibrium of ZrNi1.2Mn0.6V0.2Cr0.1 and its related hydrogenation properties. J. Alloys Compd. 1997, 248, 215–219. [Google Scholar] [CrossRef]
  241. Yang, X.G.; Lei, Y.Q.; Shu, K.Y.; Lin, G.F.; Zhang, Q.A.; Zhang, W.K.; Zhang, X.B.; Lu, G.L.; Wang, Q.D. Contribution of rare-earths to activation property of Zr-based hydride electrode. J. Alloys Compd. 1999, 293, 632–636. [Google Scholar] [CrossRef]
  242. Sun, J.C.; Li, S.; Ji, S.J. The effects of the substitution of Ti and La for Zr in ZrMn0.7V0.2Co0.1Ni1.2 hydrogen storage alloys on the phase structure and electrochemical properties. J. Alloys Compd. 2007, 446, 630–634. [Google Scholar] [CrossRef]
  243. Chen, W.X. Effects of addition of rare-earth element on electrochemical characteristics of ZrNi1.1Mn0.5V0.3Cr0.1 hydrogen storage alloy electrodes. J. Alloys Compd. 2001, 319, 119–123. [Google Scholar] [CrossRef]
  244. Jung, J.H.; Lee, K.Y.; Lee, J.Y. The activation mechanism of Zr-based alloy electrodes. J. Alloys Compd. 1995, 226, 166–169. [Google Scholar] [CrossRef]
  245. Joubert, J.M.; Sun, D.; Latroche, M.; Percheron-Guegan, A. Electrochemical performances of ZrM2 (M=V, Cr, Mn, Ni) Laves phases and the relation to microstructures and thermodynamical properties. J. Alloys Compd. 1997, 253, 564–569. [Google Scholar] [CrossRef]
  246. Han, S.M.; Zhang, Z.; Zhao, M.S.; Zheng, Y.Z. Electrochemical characteristics and microstructure of Zr0.9Ti0.1Ni1.1Mn0.6V0.3–LaNi5 composite hydrogen storage alloys. Int. J. Hydrogen Energy 2006, 31, 563–567. [Google Scholar] [CrossRef]
  247. Wang, Y.; Zhao, M.; Li, S.; Wang, L. Structure and electrochemical characteristics of melted composite Ti0.10Zr0.15V0.35Cr0.10Ni0.30–LaNi5 hydrogen storage alloys. Electrochim. Acta 2008, 53, 7831–7837. [Google Scholar] [CrossRef]
  248. Lu, Z.; Qin, M.; Jiang, W.; Qing, P.; Liu, S. Effect of AB2-based alloy addition on structure and electrochemical properties of La0.5Pr0.2Zr0.1Mg0.2Ni2.75Co0.45Fe0.1Al0.2 hydrogen storage alloy. J. Rare Earths 2013, 31, 386–394. [Google Scholar] [CrossRef]
  249. HEFA Rare Earth. Available online: http://mineralprices.com (accessed on 8 May 2017).
  250. Griessen, R.; Riesterer, T. Heat of Formation Models. In Hydrogen in Intermetallic Compounds I; Schlapbach, L., Ed.; Springer: Berlin/Heidelberg, Germany, 1988. [Google Scholar]
  251. Zhu, J.H.; Pike, L.M.; Liu, C.T.; Liaw, P.K. Point defects in Binary NbCr2 Laves-phase alloys. Scr. Mater. 1998, 39, 833–838. [Google Scholar] [CrossRef]
  252. Kanazawa, S.; Kaneno, Y.; Inoue, H.; Kim, W.Y.; Takasugi, T. Microstructures and defect structures in ZrCr2 Laves phase based intermetallic compounds. Intermetallics 2002, 10, 783–792. [Google Scholar] [CrossRef]
  253. Wong, D.F.; Young, K.; Ouchi, T.; Ng, K.Y.S. First-principles point defect models for Zr7Ni10 and Zr2Ni7 phases. Batteries 2016, 2, 23. [Google Scholar] [CrossRef]
  254. Massalski, T.B. Binary Alloy Phase Diagrams, 2nd ed.; ASM International: Russell, OH, USA, 1990. [Google Scholar]
  255. Notten, P.H.L.; Einerhand, R.E.F.; Daams, J.L.C. How to achieve long-term electrochemical cycling stability with hydride-forming electrode materials. J. Alloys Compd. 1995, 231, 604–610. [Google Scholar] [CrossRef]
  256. Young, K.; Ouchi, T.; Yang, J.; Fetcenko, M.A. Studies of off-stoichiometric AB2 metal hydride alloy: Part 1. Structural characteristics. Int. J. Hydrogen Energy 2011, 36, 11137–11145. [Google Scholar] [CrossRef]
  257. Young, K.; Nei, J.; Huang, B.; Fetcenko, M.A. Studies of off-stoichiometric AB2 metal hydride alloy: Part 2. Hydrogen storage and electrochemical properties. Int. J. Hydrogen Energy 2011, 36, 11146–11154. [Google Scholar] [CrossRef]
  258. Liu, B.H.; Li, Z.P.; Suda, S. Electrochemical cycle life of Zr-based Laves phase alloys influenced by alloy stoichiometry and composition. J. Electrochem. Soc. 2002, 149, A537–A542. [Google Scholar] [CrossRef]
  259. Zhu, Y.; Pan, H.; Gao, M.; Ma, J.; Lei, Y.; Wang, Q. Electrochemical studies on the Ti–Zr–V–Mn–Cr–Ni hydrogen storage electrode alloys. Int. J. Hydrogen Energy 2003, 28, 311–316. [Google Scholar] [CrossRef]
  260. Pan, H.; Zhu, Y.; Gao, M.; Liu, Y.; Li, R.; Lei, Y.; Wang, Q. A study on the cycling stability of the Ti–V-based hydrogen storage electrode alloys. J. Alloys Compd. 2004, 364, 271–279. [Google Scholar] [CrossRef]
  261. Yasuoka, S.; Magari, Y.; Murata, T.; Tanaka, T.; Ishida, J.; Nakamura, H.; Nohma, T.; Kihara, M.; Baba, Y.; Teraoka, H. Development of high-capacity nickel-metal hydride batteries using superlattice hydrogen-absorbing alloys. J. Power Sources 2006, 156, 662–666. [Google Scholar] [CrossRef]
  262. Young, K.; Fetcenko, M.A. Low Cost, High Power, High Energy, Solid-State, Bipolar Metal Hydride Batteries. U.S. Patent 8,974,948, 10 March 2015. [Google Scholar]
  263. Young, K.; Wong, D.; Nei, J.; Reichman, B.; Chao, B.; Mays, W. Shared Electrode Hybrid Battery-Fuel Cell System. U.S. Patent Appl. 20,150,295,290, 15 October 2015. [Google Scholar]
  264. Zelinsky, M.A.; Koch, J.M. Nickel/metal hydride batteries in stationary applications. Batteries 2017. submitted. [Google Scholar]
  265. Wikipedia. Start-Stop System. Available online: https://en.wikipedia.org/wiki/Start-stop_system (accessed on 31 July 2017).
  266. Yan, S.; Meng, T.; Young, K.; Nei, J. Nickel/metal hydride battery in a pouch design. Batteries 2017. in preparation. [Google Scholar]
  267. Young, K.; Nei, J.; Meng, T. Alkaline and Non-Aqueous Proton-Conducting Pouch-Cell Batteries. U.S. Patent Appl. 20,160,233,461, 11 August 2016. [Google Scholar]
  268. Meng, T.; Young, K.; Wong, D.F.; Nei, J. Ionic liquid-based non-aqueous electrolytes for nickel/metal hydride batteries. Batteries 2017, 2, 4. [Google Scholar] [CrossRef]
Figure 1. Schematic of (a) C14 (hexagonal), (b) C15 (cubic), (c) and C36 (rhombohedral) crystal structures [28].
Figure 1. Schematic of (a) C14 (hexagonal), (b) C15 (cubic), (c) and C36 (rhombohedral) crystal structures [28].
Batteries 03 00027 g001
Figure 2. Images of (a) a 200 g, (b) 60 kg, and (c) 1 ton vacuum induction melting (VIM) furnaces. While the first two are currently installed in BASF-Ovonic, the third one is operated by Rare-earth Ovonic Metal Hydride Alloy Company in Baotou, Inner Mongolia, China.
Figure 2. Images of (a) a 200 g, (b) 60 kg, and (c) 1 ton vacuum induction melting (VIM) furnaces. While the first two are currently installed in BASF-Ovonic, the third one is operated by Rare-earth Ovonic Metal Hydride Alloy Company in Baotou, Inner Mongolia, China.
Batteries 03 00027 g002
Figure 3. Scanning Electron Microscope (SEM) cross-section micrographs showing the microstructures from various locations of a 100-kg AB2 ingot with a composition of Ti9Zr26.2V5Cr3.5Mn15.6Co1.5Ni38Sn0.8Al0.4 prepared by VIM. The electrochemical discharge capacities of ingots from locations A, B, C, D, E, and F are 390, 400, 391, 402, 389, and 397 mAh·g−1 with a discharge current density of 8 mA·g−1. The dark, white, and gray regions are ZrO2 inclusions, secondary phases (TiNi, ZrNi, Zr7Ni10, and Zr9Ni11), and main C14 phases, respectively.
Figure 3. Scanning Electron Microscope (SEM) cross-section micrographs showing the microstructures from various locations of a 100-kg AB2 ingot with a composition of Ti9Zr26.2V5Cr3.5Mn15.6Co1.5Ni38Sn0.8Al0.4 prepared by VIM. The electrochemical discharge capacities of ingots from locations A, B, C, D, E, and F are 390, 400, 391, 402, 389, and 397 mAh·g−1 with a discharge current density of 8 mA·g−1. The dark, white, and gray regions are ZrO2 inclusions, secondary phases (TiNi, ZrNi, Zr7Ni10, and Zr9Ni11), and main C14 phases, respectively.
Batteries 03 00027 g003
Figure 4. Images of (a) an arc melter, (b) a centrifugal casting VIM, (c) a melt-spinning VIM, and (d) a gas atomizer. The first three are operated in Ovonic-BASF and the fourth one is in Eutectix, Troy, MI, USA.
Figure 4. Images of (a) an arc melter, (b) a centrifugal casting VIM, (c) a melt-spinning VIM, and (d) a gas atomizer. The first three are operated in Ovonic-BASF and the fourth one is in Eutectix, Troy, MI, USA.
Batteries 03 00027 g004
Figure 5. Images during operation of (a) a VIM, (b) a centrifugal casting (CC), (c) a gas atomization (GA) (Courtesy of Daido Steel, Nagoya, Japan).
Figure 5. Images during operation of (a) a VIM, (b) a centrifugal casting (CC), (c) a gas atomization (GA) (Courtesy of Daido Steel, Nagoya, Japan).
Batteries 03 00027 g005
Figure 6. SEM micrographs showing top morphologies of alloys prepared by (a) VIM with a mechanical crush-and-grind, (b) melt-spinning (MS), and (c) GA processes.
Figure 6. SEM micrographs showing top morphologies of alloys prepared by (a) VIM with a mechanical crush-and-grind, (b) melt-spinning (MS), and (c) GA processes.
Batteries 03 00027 g006
Figure 7. SEM cross-section micrographs from a C14-predominated alloy (Ti12Zr21.5V10Cr8.5Mn13.6Co1.5Ni32.2Sn0.3Al0.4) prepared by (a) a conventional VIM, (b) GA, and (c) MS processes. Areas 1, 2, 3, 4, and 5 in (a) are C14, C15, TiNi, body-centered-cubic (bcc), and ZrO2 phases, respectively, as determined by their compositions and crystal structures.
Figure 7. SEM cross-section micrographs from a C14-predominated alloy (Ti12Zr21.5V10Cr8.5Mn13.6Co1.5Ni32.2Sn0.3Al0.4) prepared by (a) a conventional VIM, (b) GA, and (c) MS processes. Areas 1, 2, 3, 4, and 5 in (a) are C14, C15, TiNi, body-centered-cubic (bcc), and ZrO2 phases, respectively, as determined by their compositions and crystal structures.
Batteries 03 00027 g007
Figure 8. Images of skull melting: (a) water-cooling Cu rods, (b) application of refractory outside the crucible, (c) setup of a crucible and a mold in a vacuum chamber, and (d) during operation (Courtesy of Albany Research Center, Albany, OR, USA).
Figure 8. Images of skull melting: (a) water-cooling Cu rods, (b) application of refractory outside the crucible, (c) setup of a crucible and a mold in a vacuum chamber, and (d) during operation (Courtesy of Albany Research Center, Albany, OR, USA).
Batteries 03 00027 g008
Figure 9. Images of (a) a shaker mill (Spex, Metuchen, NJ, USA) and (b) an attritor used in MA processes (Union Process, Akron, OH, USA).
Figure 9. Images of (a) a shaker mill (Spex, Metuchen, NJ, USA) and (b) an attritor used in MA processes (Union Process, Akron, OH, USA).
Batteries 03 00027 g009
Figure 10. Images of (a) a 2-kg stationary, (b) a 3-ton stationary, and (c) a 20-kg rotational hydrogen reactors. While the first one was taken in BASF-Ovonic, the rest of two were taken in Eutectix.
Figure 10. Images of (a) a 2-kg stationary, (b) a 3-ton stationary, and (c) a 20-kg rotational hydrogen reactors. While the first one was taken in BASF-Ovonic, the rest of two were taken in Eutectix.
Batteries 03 00027 g010
Figure 11. Images of (a) a 4-ton vacuum annealer, (b) a 200-kg vacuum annealer, and (c) a 10-kg flowing-hydrogen annealer. These pictures were taken in Rare-earth Ovonic Metal Hydride Company, Ovonic-BASF, and Eutectix.
Figure 11. Images of (a) a 4-ton vacuum annealer, (b) a 200-kg vacuum annealer, and (c) a 10-kg flowing-hydrogen annealer. These pictures were taken in Rare-earth Ovonic Metal Hydride Company, Ovonic-BASF, and Eutectix.
Batteries 03 00027 g011
Figure 12. Comparison of cycle life in C-sized cell from AB5 and AB2 (MF139.173, Ti12Zr21.5V10Cr8.5Mn13.6Co1.5Ni32.2Sn0.3Al0.4) alloys as negative electrode active materials. N/P denotes the ratio of capacities of negative and positive electrodes and capacity in the unit of Ah was obtained with a C/2 charge rate and a C/2 discharge rate to 0.9 V cell voltage.
Figure 12. Comparison of cycle life in C-sized cell from AB5 and AB2 (MF139.173, Ti12Zr21.5V10Cr8.5Mn13.6Co1.5Ni32.2Sn0.3Al0.4) alloys as negative electrode active materials. N/P denotes the ratio of capacities of negative and positive electrodes and capacity in the unit of Ah was obtained with a C/2 charge rate and a C/2 discharge rate to 0.9 V cell voltage.
Batteries 03 00027 g012
Figure 13. SEM cross-section micrographs of a C14 MH alloy at (a) 10th cycle, just after initial activation and (b) 450th cycle, at the end of cycle life.
Figure 13. SEM cross-section micrographs of a C14 MH alloy at (a) 10th cycle, just after initial activation and (b) 450th cycle, at the end of cycle life.
Batteries 03 00027 g013
Figure 14. X-ray energy dispersive spectroscopy Cr-mapping from MH alloys with (a) 3.5 at % Cr and 28 wt % C14, (b) 5.5 at % Cr and 53 wt % C14, and (c) 8.5 at % Cr and 87 wt % C14. The three phases are C14, C15, and ZrxNiy in order of decreasing brightness.
Figure 14. X-ray energy dispersive spectroscopy Cr-mapping from MH alloys with (a) 3.5 at % Cr and 28 wt % C14, (b) 5.5 at % Cr and 53 wt % C14, and (c) 8.5 at % Cr and 87 wt % C14. The three phases are C14, C15, and ZrxNiy in order of decreasing brightness.
Batteries 03 00027 g014
Figure 15. Plot of solubility (composition range) vs. ratio of atomic radii between A-site and B-site atoms from Ti, Zr, Hf-based Laves phase intermetallic compounds (IMCs). Red and blue dots are the upper and lower bounds of the AB2 soluble range (yellow vertical line) in the composition. Data points in red circles are from C14 phases and other unmarked data points are from C15 phases.
Figure 15. Plot of solubility (composition range) vs. ratio of atomic radii between A-site and B-site atoms from Ti, Zr, Hf-based Laves phase intermetallic compounds (IMCs). Red and blue dots are the upper and lower bounds of the AB2 soluble range (yellow vertical line) in the composition. Data points in red circles are from C14 phases and other unmarked data points are from C15 phases.
Batteries 03 00027 g015
Table 1. The performance comparison of hydrogen-absorbing alloys with different chemistries [12]. The numbers in parentheses are the nominal B/A ratios. The symbols are ++ (superb), + (good), 0 (acceptable), and − (poor).
Table 1. The performance comparison of hydrogen-absorbing alloys with different chemistries [12]. The numbers in parentheses are the nominal B/A ratios. The symbols are ++ (superb), + (good), 0 (acceptable), and − (poor).
PropertiesAB2 (2)AB3 (3)A2B7 (3.5)A5B19 (3.8)AB5 (5)
AB2 number of units11110
AB5 number of units01231
Electrochemical capacity/weight++0+0
Electrochemical capacity/volume00+0
Pulverization of alloy, oxidation (corrosion)+++
Reversibility of hydrogen absorption/release0+0~+++
Battery Life0++0+
Table 2. Comparison between alloy preparation methods. VIM, CC, MS, GA, MA, AM, and PS are short for vacuum induction melting, centrifugal casting, melt spinning, gas atomization, mechanical alloying, arc melting, and plasma spray, respectively.
Table 2. Comparison between alloy preparation methods. VIM, CC, MS, GA, MA, AM, and PS are short for vacuum induction melting, centrifugal casting, melt spinning, gas atomization, mechanical alloying, arc melting, and plasma spray, respectively.
PropertiesVIMCCMSGAMAAMPS
PurposeProductionResearch/ProductionResearch/ProductionResearch/ProductionResearchResearchResearch
Batch Size1–1000 kg1–1000 kg1–200 kg1–1000 kg1–1000 g5–200 g5–100 g
Equipment CostMediumHighHighHighLowLowHigh
Production Cost$3 kg−1$4 kg−1$4 kg−1$5 kg−1$1000 kg−1$1000–$5000 kg−1$2000 kg−1
Cooling Rate100 °C s−11 × 103 °C s−11 × 106 °C s−11 × 104 °C s−1>1 × 106 °C s−1500 °C s−11 × 104 °C s−1
Micro-structureLarge crystallitesMedium crystallitesNano-crystallitesMicro-crystallitesAmorphousLarge crystallitesMicro-crystallites
Alloy Discharge CapacityNormalNormalLowLowHighNormalLow
Alloy High-Rate Discharge-abilityNormalNormalHighLowHighNormalHigh
Alloy Cycle Stability (Anti-pulverization)NormalBetterExcellentExcellentExcellentNormalExcellent
Table 3. Performance requirements of MH alloy in various type of applications. The symbols are ++ (highly desirable), + (important), 0 (not critical), and × (unrelated). EV and HEV represent electric vehicle and hybrid electric vehicle, respectively.
Table 3. Performance requirements of MH alloy in various type of applications. The symbols are ++ (highly desirable), + (important), 0 (not critical), and × (unrelated). EV and HEV represent electric vehicle and hybrid electric vehicle, respectively.
Alloy RequirementsHigh-Energy (EV)High-Power (HEV)Stationary General PurposeStationary at High TemperatureStationary at Low Temperature
H-storage Capacity++0+++
H-diffusibility+++++++
Surface Catalysis++++++++
Anti-corrosion+0++++
Equilibrium Pressure0++0×++
Pulverization+++0++
Cost+++++++
Table 4. Calculation of leaching rate in 100 °C/30% KOH of a C14 MH alloy with a composition of Ti12Zr21.5V9.5Cr4.5Mn13.6Co2Ni36.2Sn0.3Al0.4. Data are from [87].
Table 4. Calculation of leaching rate in 100 °C/30% KOH of a C14 MH alloy with a composition of Ti12Zr21.5V9.5Cr4.5Mn13.6Co2Ni36.2Sn0.3Al0.4. Data are from [87].
ElementTiZrVAlMn
Amount in alloy (at %)12.021.59.50.413.6
Concentration in solution after 1 h etching (ppm)0.615.611.47.80.4
Concentration in solution after 4 h etching (ppm)1.048.933.828.10.5
Leaching rate after 1 h etching (ppm/at %)0.050.731.219.50.03
Leaching rate after 4 h etching (ppm/at %)0.082.273.670.20.04
Table 5. Properties of A-site elements in AB2 alloys. IMC denotes intermetallic compound.
Table 5. Properties of A-site elements in AB2 alloys. IMC denotes intermetallic compound.
PropertiesTiZrHfNbPd
Atomic Number2240724146
Atomic Radius in AB21.6141.7711.7431.6251.521
Electronegativity1.541.331.301.602.20
Earth Crust Abundance (%)0.660.0133.3 × 10−41.7 × 10−36 × 10−7
Melting Temperature (°C)16681855215024681555
ΔHh (kJ·mol H2−1)−136−164−161−83−41
Number of IMCs with Ni38830
Table 6. Properties of first-row transition metal elements as B-site atoms in AB2 alloys.
Table 6. Properties of first-row transition metal elements as B-site atoms in AB2 alloys.
PropertiesVCrMnFeCoNiCuZn
Atomic Number2324252627282930
Atomic Radius in AB21.4911.4231.4281.4111.3851.3771.4131.538
Electronegativity1.631.661.551.831.881.911.901.65
Earth Crust Abundance (%)0.0190.0140.116.30.0030.0090.0070.008
Melting Temperature (°C)1890185712451535149514531083420
ΔHh (kJ·mol H2‒1)−35−8−81015−3208
Number of IMCs with Ti01124357
Table 7. Properties of some REs used as additives in AB2 MH alloys.
Table 7. Properties of some REs used as additives in AB2 MH alloys.
PropertiesYLaCePrNdSmGdYb
Atomic Number3957585960615570
Price (US$/kg) [249]3577856075595
Ionic Radius in Laves (Å) [148]1.9903.3352.0172.0132.0131.9901.9921.990
Electronegativity1.221.101.121.131.141.171.201.24
Melting Temperature (°C)1522918798931102110721313819
Oxidation potential (V)−2.372−2.379−2.335−2.353−2.323−2.304−2.279−2.19
Heat of Hydride Formation (kJ·mol H2−1) [250]−114−97−103−104−106−100−98−91
Table 8. Influence of commonly used modifiers to C14 alloy performance. The symbols are ++ (highly beneficial), + (beneficial), 0 (no significant effect), and − (detrimental). Degree of pulverization is the combination of actual measurement [88] and estimation from PCT hysteresis and C14 phase lattice constant ratio a/c. Equilibrium pressure changes are indicated with up or down arrows.
Table 8. Influence of commonly used modifiers to C14 alloy performance. The symbols are ++ (highly beneficial), + (beneficial), 0 (no significant effect), and − (detrimental). Degree of pulverization is the combination of actual measurement [88] and estimation from PCT hysteresis and C14 phase lattice constant ratio a/c. Equilibrium pressure changes are indicated with up or down arrows.
Alloy RequirementsTiZrVCrMnFeCoNiCuZnAlSiLa
H-storage Capacity+++00/+0+000+00
H-diffusibility+0000++++
Surface Catalysis++0+++++++
Anti-corrosion+++00++00000
Equilibrium Pressure↑↑↓↓↓↓↓00000
Anti-pulverization+00000+0
Cost00+++++0+++++++++
Table 9. Solubility (range of A-site atom concentration in at %) of Laves phase IMCs (radius from [148] and solubility from [257]).
Table 9. Solubility (range of A-site atom concentration in at %) of Laves phase IMCs (radius from [148] and solubility from [257]).
IMCStructureRA/RBSolubility (at%)
ZrV2C151.1933.3
HfV2C151.1733.5–34.5
TiCr2C151.1335–37
ZrCr2C151.2431–36
HfCr2C151.2233–35
TiMn2C141.1330–40
ZrMn2C141.2420.8–40
HfMn2C141.2225.5–38
TiMn2C141.1427.5–35.5
ZrMn2C151.2627.1–34
HfMn2C151.2432–33.5
TiCo2C151.1733–33.5
ZrCo2C151.2827–35
HfCo2C151.2627–36

Share and Cite

MDPI and ACS Style

Young, K.-H.; Chang, S.; Lin, X. C14 Laves Phase Metal Hydride Alloys for Ni/MH Batteries Applications. Batteries 2017, 3, 27. https://doi.org/10.3390/batteries3030027

AMA Style

Young K-H, Chang S, Lin X. C14 Laves Phase Metal Hydride Alloys for Ni/MH Batteries Applications. Batteries. 2017; 3(3):27. https://doi.org/10.3390/batteries3030027

Chicago/Turabian Style

Young, Kwo-Hsiung, Shiuan Chang, and Xinting Lin. 2017. "C14 Laves Phase Metal Hydride Alloys for Ni/MH Batteries Applications" Batteries 3, no. 3: 27. https://doi.org/10.3390/batteries3030027

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop