Article

Investigation on Crystallization and Magnetic Properties of (Nd, Pr, Ce)2Fe14B/α-Fe Nanocomposite Magnets by Microwave Annealing Treatment

1
Department of Materials Science and Engineering, Shanghai Institute of Technology, Shanghai 201418, China
2
Department Key Laboratory for Advanced Metals and Materials, University of Science and Technology Beijing, Beijing 100083, China
*
Authors to whom correspondence should be addressed.
Materials 2021, 14(11), 2739; https://doi.org/10.3390/ma14112739
Submission received: 13 March 2021 / Revised: 18 May 2021 / Accepted: 20 May 2021 / Published: 22 May 2021

Abstract

:
In the present work, the structures and magnetic properties of (Nd, Pr, Ce) 2Fe14B/α-Fe nanocomposite magnets were thoroughly investigated. The microwave annealing was applied to achieve a uniform heating effect and uniform grains. Microwave annealing is more favorable to obtain α-Fe phase than conventional annealing, which leads to the enhanced coercivity of hysteresis loops. The coercivity of nanocomposite magnets was 245 kA/m after annealing at 2000 W for 10 min.

1. Introduction

Nd2Fe14B/α-Fe nanocomposite magnets have attracted considerable research attention owing to the highest theoretical maximum energy product [1,2,3]. As previously reported, adjustment of the alloy composition and control of the crystallization process, especially the substitution of the Fe and Nd elements [4,5,6] was applied to improve the microstructure and properties [7,8]. Many elements (such as Pr, Y, etc.) have been applied to tailor the grain size and the crystallization phase [9,10,11]. As two effective rare earth elements, Pr and Ce have been widely used to substitute the Fe and Nd elements of Nd2Fe14B/α-Fe nanocomposite magnets and adjust their magnetic properties. Pr2Fe14B and Ce2Fe14B have the same crystal structure as the Nd2Fe14B, and the replacement of Ce element to Nd is beneficial to reduce the cost of RE-Fe-B magnets [12]. Nevertheless, the substitution of Ce for Nd deteriorates the magnetic properties because of the formation of Ce2Fe14B with low intrinsic magnetic properties [13], so in this research, the addition of Pr element is necessary, because the Pr substitution for the Nd improves the hard magnetic properties of the nanocomposite magnets [14]. The magnetic properties are significantly improved after the substitution of Ce and Pr elements to Nd [15]. Diffusion-processing is the typical method to fabricate high magnetic performance Nd-Pr-Ce-Fe-B sintered magnets [16]. For nanocomposite magnets with Ce and Pr substitution, the uniform and fine microstructure become the critical factor in improving the magnetic properties.
As is well known, the optimization of the annealing process is one of the effective ways to obtain uniform and fine microstructure of nanocomposite magnets [17,18]. The microwave heating process has shown significant advantages against conventional heating procedures in structure controlling. Microwave heating can heat materials to high temperatures with ultra-fast heating rates, short time, and high energy efficiency [19,20,21,22,23,24]. A higher heating rate favors obtaining uniform and refined grains after the crystallization process [25], enhancing coercivity, and also adjusts the proportion of hard and soft phases. Thus, the application of microwave annealing may show great benefit for the improvement of magnetic properties of Nd2Fe14B/α-Fe nanocomposite magnets.
The contributions of our research are highlighted as follows: we crystallized amorphous (Nd, Pr, Ce)2Fe14B/α-Fe nanocomposite ribbons by microwave heating treatment and investigated their magnetic properties, which has rarely been reported before.

2. Materials and Methods

2.1. Materials

The ingots with nominal composition (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons were prepared by arc-melting under a high-purity Ar atmosphere. The sizes of small pieces of ingots are 5–7 mm, they were re-melted and spun onto a copper roll, and the wheel speed 22 m/s.

2.2. Methods

To study the effect of microwave-assisted annealing on crystallization, we used a quartz tube with a vacuum of 5 × 10−3 Pa to seal the as-spun ribbons, and apply direct microwaves on ribbons at 650 °C for 10 min under the power of 800, 1500, and 2000 W, respectively. The HAMiLab-V3 microwave furnace (Beijing Yiye Lantian Technology Co., Ltd., Beijing, China) with a frequency of 2.45 GHz is experimental equipment. The (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons were heated at a rate of 5, 20, and 40 °C/min. We used a differential scanning calorimeter (DSC, (Shanghai Precision Scientific Instrument Co., Ltd., Shanghai, China) to characterize the as-spun ribbons, and X-ray diffraction (XRD) with Cu-Kα radiation to determine the structure of the as-spun and annealed ribbons. A vibrating sample magnetometer (VSM, (YP Magnet Technology Development Co., Ltd.) is used to measure the magnetic properties of the ribbons with a maximum applied magnetic field of 1.8 T.

3. Results and Discussion

3.1. Crystallization Process

The XRD pattern of (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons is shown in Figure 1. No distinct diffraction peaks were found in the patterns, the broad peak in the interval 35–50 degrees is due to the amorphous phase.
The DSC curves of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons at a heating rate of 5, 20, and 40 °C/min are shown in Figure 2. Only one exothermic peak is detected, which indicates the synchronized precipitation of soft and hard magnetic phases, and they were formed at the same temperature. The crystallization characteristic temperature increased with the increase of the heating rate due to the hysteresis effect of phase change and the superheat. Moreover, as the heating rate increased, the higher the phase change energy storage per unit time was, the higher the heat released during the phase change was, so the exothermic peak became larger. Activation energy during the crystallization is a crucial parameter of thermal stability for the amorphous alloy, which statistically reflects the average of the activation energy in the crystallization process. The crystallization tendency of the amorphous alloy decreases with the increase of effective activation energy. According to Kissinger equation [26]:
I n T 2 B = E R T + C
where I n is natural logarithm; B is the heating rate; T is the characteristic crystallization temperature (in this study, we select T = Tp); E is the crystallization activation energy; R is the molar gas constant; and C is constant. The linear relationship between T 2 B and 1 T is shown in Figure 3. The slope values of E/R represent crystallization activation energy, resulting from E = 121.1 KJ/mol.

3.2. Comparison of Conventional Annealing and Microwave Annealing

The XRD patterns of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons annealed at 650 °C for 10 min under conventional and microwave heating conditions, respectively, are shown in Figure 4. Apart from the diffraction peaks from (Nd, Pr, Ce)2Fe14B and α-Fe phases, a broad peak locates from 20 degrees to 25 degrees is detected, suggesting the presence of some amorphous phases after conventional annealing treatment. However, the ribbons were annealed by microwave by increasing the microwave power from 800 W to 2000 W, the intensity of the α-Fe peak became significantly stronger than the (Nd, Pr, Ce)2Fe14B peak. The grain size can be calculated from the line width (FWHM in radian) of XRD [27]. It shows that with the increase of microwave power, the grain size of the α-Fe phase increased greatly; however, the grain size of the (Nd, Pr, Ce)2Fe14B phase increased slightly, as are shown in Table 1, because microwave annealing treatment promotes the diffusion of elements, accelerates the crystallization rate, and then promotes the growth of grains, especially the α-Fe phase. The average size of grains increases from 11.9 nm in traditional annealing to 40.3 nm in microwave annealing at 2000 W. It explained that the microwave annealing treatment increased the grain size. Moreover, the broad peak completely disappears, presenting the elimination of the residual amorphous phase. The desired microstructural modifications have been achieved in the (Nd, Pr, Ce)2Fe14B/α-Fe samples after microwave annealing for the full range of power. The diffusion rates of the elements were promoted by a microwave field, the proportion of hard and soft magnetic phases were adjusted as well.
The hysteresis loop curves of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons annealed at 650 °C for 10 min under conventional heating and microwave heating under different powers are shown in Figure 5. Their hysteresis loops display low magnetic properties. As reported, the Ce2Fe14B phase presents a lower first-order anisotropy constant than the Nd2Fe14B phase at room temperature, which induced the decrease of coercivity [28,29,30]. Even though it is expected that microwave heat treatment will increase the residual magnetization, there is no significant residual magnetic enhancement effect, and there is a weak exchange coupling effect between the soft and hard magnetic phases. The coercivity was enhanced with higher microwave power. It shows that the ribbons’ coercivity and remanence magnetic ratio under microwave annealing treatment with a power of 2000 W reaches 245 kA/m and 0.34, which are higher than that of conventional annealing (132 kA/m and 0.26), as are shown in Table 2.
The X-ray diffraction patterns of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons annealed for 5, 10, and 15 min at a microwave power of 2000 W, as are, respectively, shown in Figure 6. With the increase of crystallization time, the intensity of the pattern peaks has an increasing tendency. It shows that the grain size of the α-Fe phase increased greatly; however, the grain size of the (Nd, Pr, Ce)2Fe14B phase increased slightly, as is shown in Table 3. This is because the elements are difficult to fully diffuse in a short crystallization time, so the grains did not have enough time to grow. When annealing for 5 min, the average grain size of the α-Fe phase is only 26.9 nm. However, when the crystallization time is longer, the elements can fully diffuse, which promotes the grain growth; when annealing for 15 min, the average grain size of the α-Fe phase reached 60.2 nm. It indicated that the crystallization time affected the grain size and adjustment of the percentage of soft and hard magnetic phases.
The hysteresis loop curves of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons annealed for 5, 10, and 15 min at a microwave power of 2000 W, are, respectively, shown in Figure 7. It shows that annealing under the microwave power of 2000 W for 10 min could obtain a higher coercivity and residual magnetization, 245 kA/m and 21 Am2/kg, as are, respectively, shown in Table 4. There is no significant residual magnetic enhancement effect, and there is a weak exchange coupling effect between the soft and hard magnetic phases annealing under the microwave power of 2000 W for 10 min. The coercivity and remanent magnetic ratio could be enhanced under appropriate microwave annealing process.

4. Conclusions

This study investigated the crystallization and magnetic properties of (Nd, Pr, Ce)2Fe14B/α-Fe nanocomposite magnets through microwave annealing treatment. The results of the experiment indicate that compared with traditional annealing, even though microwave annealing slightly reduces the magnetic saturation strength of the magnet, it increases the coercivity and remanence ratio of (Nd, Pr, Ce)2Fe14B/α-Fe nanocomposite magnets. Coercivity and remanence ratio up to 245 kA/m and 0.38 for (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons were obtained after annealed at microwave field with 2000 W for 10 min.

Author Contributions

Conceptualization, Z.W. (Zhanyong Wang); methodology, C.S., M.L., Y.S. and T.W.; investigation, C.S., L.W., Z.W. (Zemin Wang) and T.W.; data analysis, C.S., L.W, Y.S. and T.W.; writing—original draft preparation, C.S. and T.W.; writing—review and editing, T.W., Z.W. (Zemin Wang), L.W. and M.L.; funding acquisition, M.L., Y.S. and Z.W. (Zhanyong Wang); supervision, Z.W. (Zemin Wang), Z.W. (Zhanyong Wang). All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the Project of the State Key Laboratory for Advanced Metals and Materials of PR China (2018-Z05) and the Shanghai Science and Technology Committee of PR China (16090503600, 19YF1446600).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

No new data were created or analyzed in this study. Data sharing is not applicable to this article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Ryo, H.S.; Hu, L.X.; Kim, J.G. Micromagnetic study for magnetic properties of exchange coupled nanocomposite magnetic systems with Nd2Fe14B grains embedded in α-Fe matrix. J. Magn. Magn. Mater. 2017, 426, 46–52. [Google Scholar] [CrossRef]
  2. Yu, X.Q.; Yue, M.; Liu, W.Q.; Li, Z.; Zhu, M.G.; Dong, S.Z.J. Structure and intrinsic magnetic properties of MM2Fe14B (MM = La, Ce, Pr, Nd) alloys. Rare Earths 2016, 34, 614–617. [Google Scholar] [CrossRef]
  3. Li, H.L.; Li, W.; Zhang, Y.M.; Gunderov, D.V.; Zhang, X.Y. Phase evolution, microstructure, and magnetic properties of bulk Alpha-Fe/Nd2Fe14B nanocomposite magnets prepared by severe plastic deformation and thermal annealing. J. Alloys Compd. 2015, 651, 434–439. [Google Scholar] [CrossRef]
  4. Wang, Z.Y.; Liu, W.Q.; Zhou, B.X.; Ni, J.S.; Xu, H.; Li, Q. Microstructural characteristics of Nd2Fe14B/α-Fe nanocomposite ribbons bearing Nb element. Rare Metals 2008, 27, 299–302. [Google Scholar] [CrossRef]
  5. Wang, H.Y.; Zhao, F.A.; Chen, N.X.; Liu, G. Theoretical investigation on the phase stability of Nd2Fe14B and site preference of V, Cr, Mn, Zr, and Nb. J. Magn. Magn. Mater. 2005, 295, 219–229. [Google Scholar] [CrossRef]
  6. Yamamoto, H.; Takahashi, K.; Hamano, R. Magnetic properties of low Rare-Earth composition Pr–Fe–Co–Ti–Nb–B system exchange-spring magnets. J. Alloys Compd. 2006, 408, 1417–1421. [Google Scholar] [CrossRef]
  7. Hussain, M.; Zhao, L.Z.; Zhang, C.; Jiao, D.L.; Zhong, X.C.; Liu, Z.W. Composition-Dependent magnetic properties of melt-spun La or/and Ce substituted nanocomposite NdFeB alloys. Phys. B 2016, 483, 69–74. [Google Scholar] [CrossRef]
  8. Wang, X.C.; Zhu, M.G.; Li, W.; Zheng, L.Y.; Guo, Z.H.; Du, X.; Du, A.; Wang, X.C.; Zhu, M.G. Effects of the ingot phase transition on microstructure and magnetic properties of CeNdFeB Melt-Spun ribbons. Phys. B 2015, 476, 255–258. [Google Scholar] [CrossRef]
  9. Yao, Q.R.; Shen, Y.H.; Yang, P.C.; Zhou, H.Y.; Rao, G.H.; Deng, J.Q.; Wang, Z.M.; Zhong, Y. Crystal structure and phase relations of Pr2Fe14B-La2Fe14B system. J. Rare Earths 2016, 34, 1121–1125. [Google Scholar] [CrossRef]
  10. Zhan, Y.Y.; Pan, J.; Jiang, X.L.; Liu, X.C.; Dong, Y.R.; Xiao, X.Y. Microstructure evolution and magnetic properties of the Nd9Fe81-xTi4C2Nb4Bx (x=11, 13, 15) bulk magnets prepared by copper mold suction casting. J. Rare Earths 2015, 33, 1081–1086. [Google Scholar] [CrossRef]
  11. Susner, M.A.; Conner, B.S.; Saparov, B.I.; McGuire, M.A.; Crumlin, E.J.; Veith, G.M.; Huibo Cao, H.B.; Shanavas, K.V.; Parker, D.S.; Zhang, Y.J. Flux growth and characterization of Ce-Substituted Nd2Fe14B single crystals. J. Magn. Magn. Mater. 2017, 434, 1–9. [Google Scholar] [CrossRef] [Green Version]
  12. Jiang, Q.; Zhong, Z. Research and development of Ce-Containing Nd2Fe14B-type alloys and permanent magnetic materials. J. Mater. Sci. Technol. 2017, 33, 1087–1096. [Google Scholar] [CrossRef]
  13. Chen, Z.; Lim, Y.K.; Brown, D. Substitution of Ce for (Nd, Pr) in Melt-Spun (Nd, Pr)–Fe–B Powders. IEEE Trans. Magn. 2015, 51, 1–4. [Google Scholar] [CrossRef]
  14. Zhang, W.-Y.; Zhang, S.-Y.; Yan, A.-R.; Zhang, H.-W.; Shen, B.-G. Effect of the substitution of Pr for Nd on microstructure and magnetic properties of nanocomposite Nd2Fe14B/α-Fe magnets. J. Magn. Magn. Mater. 2001, 225, 389–393. [Google Scholar] [CrossRef]
  15. Wei, T.; Guozhi, X. Effects of the Annealing Process on the Microwave Properties of Quenched Nd-Fe-B Alloys. In Proceedings of the 2nd International Conference on Intelligent Materials and Mechatronics(IMM 2015) and 2nd International Conference on Solar Energy Materials and Energy Engeering(SEMEE 2015), Hong Kong, China, 29 October 2015; pp. 143–147. [Google Scholar]
  16. Zhang, Y.J.; Ma, T.Y.; Yan, M.; Jin, J.Y.; Liu, X.L.; Xu, F.; Miao, X.F.; Liu, X.L. Squareness factors of demagnetization curves for multi-main-phase Nd-Ce-Fe-B magnets with different Ce contents. J. Magn. Magn. Mater. 2019, 487. [Google Scholar] [CrossRef]
  17. Zhang, Y.F.; Han, J.Z.; Liu, S.Q.; Wan, F.M.; Tian, H.D.; Zhang, X.D.; Wang, C.S.; Yang, J.B.; Yang, Y.C. Coercivity enhancement by grain refinement for anisotropic Nd2Fe14B-type magnetic powders. Scr. Mater. 2016, 110, 57–60. [Google Scholar] [CrossRef]
  18. Oghbaei, M.; Mirzaee, O. Microwave versus conventional sintering: A review of fundamentals, advantages, and applications. J. Alloys Compd. 2010, 494, 175–189. [Google Scholar] [CrossRef]
  19. Xu, R.; He, J.; Li, W.; Paine, D.C. Performance enhancement of amorphous Indium-Zinc-Oxide Thin-Film transistors by microwave annealing. Appl. Surf. Sci. 2015, 357, 1915–1919. [Google Scholar] [CrossRef]
  20. Cichoň, S.; Machác, P.; Fekete, L.; Lapcák, L. Direct microwave annealing of SiC substrate for rapid synthesis of quality epitaxial graphene. Carbon 2016, 98, 441–448. [Google Scholar] [CrossRef]
  21. Mirzaei, A.; Neri, G. Microwave-assisted synthesis of metal oxide nanostructures for gas sensing application: A review. Sens. Actuat B Chem. 2016, 237, 749–775. [Google Scholar] [CrossRef]
  22. Swaminathan, V.; Deheri, P.K.; Bhame, S.D.; Ramanujan, R.V. Novel microwave assisted chemical synthesis of Nd2Fe14B hard magnetic nanoparticles. Nanoscale 2013, 5, 2718–2725. [Google Scholar] [CrossRef]
  23. Sun, Y.; Jin, M.; Wang, Z.Y.; Jiang, H. Microwave Sintering of High Performance Strontium Ferrite Magnets and Their Magnetic Properties. J. Synth. Cryst. 2013, 42, 751–755. [Google Scholar]
  24. Gjoka, M.; Neil, D.; Hadjipanayis, G.; Niarchos, D.G. Experimental Proof of Microwave Sintering of Nd–Fe–B Powders Toward Fabrication of Permanent Magnets. IEEE Trans. Magn. 2014, 50, 1–4. [Google Scholar] [CrossRef]
  25. Wang, T.P.; Tian, T.; Ding, S.; Wang, Z.Y.; Ni, Q.X.; Zhou, D.; Dong, G.L.; Sui, Y.L.; Jin, M.L. Effects of Microwave-Assisted Annealing on the Structure and Magnetic Properties of (Nd0.75Pr0.25)9Fe72Ti1Zr3MnxMo4-xB10.5C0.5 Amorphous Ribbons. J. Supercond. Nov. Magn. 2018, 31, 2241–2246. [Google Scholar] [CrossRef]
  26. Blaine, R.L.; Kissinger, H.E. Homer Kissinger, and the Kissinger equation. Thermochim. Acta. 2012, 540, 1–6. [Google Scholar] [CrossRef]
  27. Zhou, X.D.; Huebner, W. Size-induced lattice relaxation in CeO2 nanoparticles. Appl. Phys. Lett. 2001, 79, 3512. [Google Scholar] [CrossRef]
  28. Hirosawa, S.; Matsuura, Y.; Yamamoto, H.; Fujimura, S.; Sagawa, M.; Yamauchi, H. Single crystal measurements of anisotropy constants of R2Fe14B (R = y, Ce, Pr, Nd, Gd, Tb, Dy and Ho). Jpn. J. Appl. Phys. 1985, 24, 803–805. [Google Scholar] [CrossRef]
  29. Herbst, J.F.; Hector, L.G. A computational quest for Nd2Fe14B-type Ce and Nd phases. J. Alloys Compd. 2017, 693, 238–244. [Google Scholar] [CrossRef]
  30. Yang, M.N.; Wang, H.; Hu, Y.F.; Yang, L.Y.M.; Maclennan, A.; Yang, B. Increased coercivity for Nd-Fe-B melt spun ribbons with 20 at.% Ce addition: The role of compositional fluctuation and Ce valence state. J. Alloys Compd. 2017, 710, 519–527. [Google Scholar] [CrossRef]
Figure 1. X-ray diffraction pattern of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons.
Figure 1. X-ray diffraction pattern of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons.
Materials 14 02739 g001
Figure 2. DSC curves of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons.
Figure 2. DSC curves of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons.
Materials 14 02739 g002
Figure 3. Kissinger curve of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons.
Figure 3. Kissinger curve of the (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 as-spun ribbons.
Materials 14 02739 g003
Figure 4. X-ray diffraction patterns of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different conditions.
Figure 4. X-ray diffraction patterns of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different conditions.
Materials 14 02739 g004
Figure 5. Hysteresis loop curves of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different conditions.
Figure 5. Hysteresis loop curves of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different conditions.
Materials 14 02739 g005
Figure 6. X-ray diffraction patterns of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for different time.
Figure 6. X-ray diffraction patterns of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for different time.
Materials 14 02739 g006
Figure 7. Hysteresis loop curves of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for a different time.
Figure 7. Hysteresis loop curves of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for a different time.
Materials 14 02739 g007
Table 1. The average crystallites size of the main phases of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different power applied.
Table 1. The average crystallites size of the main phases of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different power applied.
Power AppliedD (nm)
α-Fe(Nd, Pr, Ce)2Fe14B
conventional11.99.6
800 W17.712.3
1500 W25.312.9
2000 W41.318.6
Table 2. The magnetic properties of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different annealing conditions.
Table 2. The magnetic properties of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons under different annealing conditions.
Annealing Conditionsσs (Am2/kg)σr (Am2/kg)Hc (kA/m)σrs
conventional78201320.26
800 W65201350.31
1500 W65202420.31
2000 W61212450.34
The σs is remanence magnetic, σr is saturation value of magnetization, Hc is coercivity, and σrs is remanence magnetic ratio.
Table 3. The average crystallites size of the main phases of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for a different time.
Table 3. The average crystallites size of the main phases of the microwave annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for a different time.
Annealing Time (min)D (nm)
α-Fe(Nd, Pr, Ce)2Fe14B
526.911.7
1041.318.6
1560.222.4
Table 4. The magnetic properties of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for a different time.
Table 4. The magnetic properties of the annealed (Nd0.525Pr0.175Ce0.3)9Fe64.5Co3Cu0.5Ti1B22 ribbons for a different time.
Annealing Times (min)σs (Am2/kg)σr (Am2/kg)Hc (kA/m)σr/σs
581211270.27
1061232450.38
1574181190.24
The σs is remanence magnetic, σr is saturation value of magnetization, Hc is coercivity, and σr/σs is remanence magnetic ratio.
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Wang, Z.; Shangguan, C.; Wang, Z.; Wang, T.; Wang, L.; Liu, M.; Sui, Y. Investigation on Crystallization and Magnetic Properties of (Nd, Pr, Ce)2Fe14B/α-Fe Nanocomposite Magnets by Microwave Annealing Treatment. Materials 2021, 14, 2739. https://doi.org/10.3390/ma14112739

AMA Style

Wang Z, Shangguan C, Wang Z, Wang T, Wang L, Liu M, Sui Y. Investigation on Crystallization and Magnetic Properties of (Nd, Pr, Ce)2Fe14B/α-Fe Nanocomposite Magnets by Microwave Annealing Treatment. Materials. 2021; 14(11):2739. https://doi.org/10.3390/ma14112739

Chicago/Turabian Style

Wang, Zhanyong, Changping Shangguan, Zemin Wang, Tianpeng Wang, Lianbo Wang, Min Liu, and Yanli Sui. 2021. "Investigation on Crystallization and Magnetic Properties of (Nd, Pr, Ce)2Fe14B/α-Fe Nanocomposite Magnets by Microwave Annealing Treatment" Materials 14, no. 11: 2739. https://doi.org/10.3390/ma14112739

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop