1. Introduction
Vanadium is used to produce steel with rust-resistant elements and as a carbide stabilizer in the manufacture of steel, especially for nuclear applications. About 80% of the vanadium produced is used as an additive for stainless steel or ferranadium. For titanium steel plating, vanadium foil was used as a bonding agent. Vanadium pentoxide is used as a catalyst, as a mordant for dyeing and printing fabrics, in the manufacture of aniline black, and in the ceramics industry. Vanadium-gallium tape is used to produce superconducting magnets [
1].
Vanadium can be found in about 65 minerals, including vanadinite (Pb5(VO4)3Cl), carnotite (K2(UO2)2(VO4)2·3H2O), patronite (VOSO4), and roscoelite (K(V3+,Al,Mg)2AlSi3O10(OH)2). In addition, vanadium can be found in certain iron and phosphate ores and in some crude oils as organic complexes. Vanadium is found in small percentages in meteorites. Vanadium is an important component of catalysts for oxidation reactions.
Typical applications of vanadium (V) are as a catalyst for SO
2 oxidation, for the oxidation of propane and propene to acrylic acid [
2,
3,
4], for oxidative dehydrogenation of butane [
5], or for oxidation of butane to maleic anhydride [
6]. It is also used for the selective catalytic reduction of NO
x from ammonia [
7]. BiVO
4 can also be used as a catalyst for the electrochemical synthesis of H
2O
2 [
8].
Different vanadium compounds were founded in relatively low amounts in living organisms, being distributed in the bones, liver, and kidney [
9]. In this context, polyoxidovanadates present pharmacological action, being tested as anticancer, antiprotozoal, antidiabetic, antibacterial, and antiviral drugs [
10,
11,
12]. Starting from such research becomes evident that the proper disposal and further recovery of the vanadium ions from expired drugs are required.
As a result of all of these applications, relatively large amounts of vanadium (V) are accumulated in various industrial wastes. Given the value of vanadium (V), from an economic point of view, recovery has become a necessity. Various processes are being developed for this purpose. Recovery options include hydrometallurgical operations, such as leaching, purification of the solution by solvent extraction, and precipitation, and pyrometallurgical operations, such as direct melting and frying [
13]. Ionic exchange could be another option for recovery [
14].
A material has good adsorbent properties if it presents a high adsorption capacity, the smallest pore diameter, the largest specific surface area, and the possibility of high regeneration. Among the usual materials used are activated carbon, silica gel, alumina, zeolites, polymer matrix, etc. [
15,
16,
17].
The goal of this study is to synthesize new materials that can have tuned properties based on silica and iron oxide. We obtained a SiO
2Fe
xO
y xerogel, which we further used to recover the vanadium from waste water by adsorption, indicating good results. This adsorbent material was chosen because similar material was used for recovery of different metallic ions, presenting an interesting behaviour. Another reason is represented by the presence of vanadium ions in red blood cells [
9,
11,
18], which allows us to think that presence of iron can improve the adsorptive properties of this material.
2. Materials and Methods
2.1. Material Synthesis
Following previous work [
19], SiO
2Fe
xO
y xerogel is synthesized using the sol-gel method, using tetraethyl-orthosilicate-TEOS, Si (OC
2H
5)
4, (SigmaAldrich) (7 mL) as silica precursors and iron (II) acetylacetonate, C
10H
14FeO
4, Fe(acac)
2 (SigmaAldrich, Burlington, MA, USA) (0.54 g) as iron oxide precursors. The TEOS is dissolved in 37.2 mL of ethanol (Chimopar, SC CHIMOPAR TRADING SRL, Bucharest, Romania) and stirred for 10 min at 500 rpm using a magnetic stirrer (DLAB MS-HS); then, 13.8 mL of deionised water is added and stirred for 30 more minutes. Iron (II) acetylacetonate is also added, stirring mechanically for 3 h and maintaining a temperature of 55 °C in the solution. Gels are formed when NH
3 (Chimopar, SC CHIMOPAR TRADING SRL) (0.46 g) is used as catalyst, with the pH becoming 10. Obtained material is left for 24 h to age at room temperature and then dried in an oven (POL-EKO SLW53, Poland) at 100 °C for 24 h.
A schematic presentation of the synthesis is shown in
Figure 1.
2.2. Material Characterization
Knowledge regarding material crystallinity degree, but also about the existence of several phases in the material, X-ray diffraction (XRD) analysis was performed using the Ultima IV instrument (RIGAKU) operating with Co-Kα radiation. N2 adsorption–desorption isotherm is obtained using the Nova 1200e Quantachrome apparatus. Furthermore, the newly prepared material was characterized by scanning electron microscopy (SEM) coupled with energy dispersive X-ray spectroscopy (EDX, Cambridge, MA, USA), employing the FEI Quanta FEG 250 scanning electron microscope.
2.3. Studies on the Recovery of Vanadium (V) Ions by Adsorption onto SiO2FexOy Material
2.3.1. Effect of the S:L Ratio
To establish the S:L ratio at which the best recovery efficiency of vanadium (V) takes place, the amount of adsorbent material, SiO2FexOy (0.05; 0.1; 0.2; 0.3; 0.4; and 0.5), was varied, maintaining the constant volume of solution (25 mL) of ammonium metavanadate, NH4VO3 (Merck, Darmstadt, Germany), containing 50 mg Vanadium (V)/L. Adsorption was accomplished in a Julabo SW23 shaker with thermostat and stirring, where the samples are kept in contact for 60 min at 298 K and 200 rpm.
Vanadium (V) analysis was performed by UV-VIS spectroscopy using the Varian Carry 50 spectrometer. Then, 2.5 mL of sample solution was added to 1 mL of H2SO4 6 N (CHEMICAL Company), 1 mL of H3PO4 6 N (Sigma Aldrich) and 0.5 mL of Na2WO4 solution (Merck) (8.25 g of Na2WO4 in 50 mL of water). The spectra were recorded at a wavelength of 400 nm.
2.3.2. pH Effect
To determine the pH influence on the vanadium adsorption process on the adsorbent material, 0.1 g of material, SiO2FexOy, was kept in contact for 60 min at a temperature of 298 K with 25 mL of solution at initial concentration, C0 = 50 mg V (V)/L. Solutions’ pH values were adjusted using solutions of HNO3 (63%, Carl Roth) and NaOH (Sigma Aldrich) solutions with concentrations in the range of 0.1–1 N.
2.3.3. Contact Time and Temperature Effect
To study the influence of temperature and contact time on the adsorption capacity of the adsorbent material, 0.1 g of material was accurately weighed and over 25 mL of vanadium solution of initial concentration C0 = 50 mg/L were added. Using a water bath with thermostat and stirring, the xerogel sample was first stirred at 200 rpm for 15, 30, 60, and 120 min at three different temperatures, namely 298 K, 308 K, and 318 K.
2.3.4. Kinetic Studies
The kinetic equations used to investigate kinetics of the vanadium adsorption process are presented in
Table 1.
2.3.5. Activation Energy, Ea
The activation energy E
a was calculated using the Arrhenius equation and the speed constant from the pseudo- second order kinetic model k
2 is represented graphically by ln k
2 = f (1/T).
where: k
2—Speed constant, g/min∙mg
A—Arrhenius constant, g∙min/mg
Ea—Activation energy, kJ/mol
T—Absolute temperature, K
R—The ideal gas constant, 8.314 J/mol∙K.
The activation energy, Ea, will give us the information needed to describe the nature of the adsorption process.
2.3.6. Thermodynamic Studies
The temperature range of 298–318 K was selected to evaluate the thermodynamic studies by calculating the free energy using the Gibbs-Helmholtz equation [
15]:
where: ΔG
0—standard Gibbs free energy variation, kJ/mol
ΔH0—standard enthalpy variation, kJ/mol
ΔS0—standard entropy variation, J/mol∙K
T—absolute temperature, K.
Using the van’t Hoff equation obtained from the linear representation of ln K
d = f (1/T), the standard variation of the entropy ΔS
0 and the standard variation of the enthalpy ΔH
0 can be calculated.
where: K
d—equilibrium constant
ΔS0—standard entropy variation, J/mol∙K
ΔH0—standard enthalpy variation, kJ/mol
R—the ideal gas constant, 8.314 J/mol∙K.
The equilibrium constant is the ratio between the adsorption capacity at equilibrium q
e and the equilibrium concentration C
e.
The plot ln Kd = f (1/T) will be represented.
2.3.7. Initial Concentration Effect
To determine the effect of the initial Vanadium (V) concentration on the adsorption capacity of the SiO2FexOy material, V (V) solutions of different concentrations, namely 25, 50, 75, 100, 120, 160, 200, 300, 400, 500, and 600 mg/L were prepared. These were obtained by an appropriate dilution from a stock solution of ammonium metavanadate, NH4VO3, 1000 mg/L. Adsorption was performed at the ratio S:L = 0.1 g:25 mL, pH = 2, contact time 60 min and at a temperature of 298 K.
2.3.8. Equilibrium Studies
To establish the adsorption mechanism, three isotherms were used, namely Langmuir, Freundlich, and Sips (
Table 2).
2.3.9. Desorption Studies
The reprocessing of absorbents is an important economic factor. At the same time, obtaining a solution with concentrated vanadium (V) is essential for further applications. Therefore, adsorption–desorption studies have been performed to investigate the potential for reuse of SiO2FexOy material. Initially, adsorption studies were performed at equilibrium, when 25 mL of vanadium solution (having initial concentration of 400 mg/L) were mixed with 1 g of adsorbent material at pH = 2, contact time 90 min and 298 K. Desorption experiments were performed using 50 mL of NaNO3 (Carl Roth) 5 M, and also NaCl (Merck, Germany) 5 M solutions, which were mixed with exhausted adsorbent material for 120 min. After time has elapsed, the desorbed vanadium content has been analysed.
3. Resultants and Discussion
3.1. Characterization of the Synthesized Material
3.1.1. X-ray Diffraction (XRD)
Figure 2 shows the spectrum obtained for SiO
2Fe
xO
y material.
The following databases were taken into account for the identification of the main phases in the material: JCPDS:9006316 specifics for the cubic phase Fd3m of maghemite, JCPDS:00-030-1762 specific for the orthorhombic phase for acetyl iron acetone II, and JCPDS:1011172 for amorphous silica.
The XRD diffractogram of the synthesized material shown in
Figure 2 generally indicates an amorphous aspect of the sample. The diffraction lines specific to SiO
2 observed at 20–30 2θ overlap with those specific to Fe(acac)
2. Detailed analysis of the recorded spectrum also shows the appearance of diffraction lines at 35, 43, 57, 63 2θ, specific to the formation of γ-Fe
2O
3 but in a very small amount. According to Scherrer’s calculation, it was found that the γ-Fe
2O
3 particles were an average size of 20 nm.
3.1.2. N2 Sorption Analysis
The determination of porosity is based on the measurement of the amount of gas (usually N2) adsorbed or desorbed on the surface of solids, porous or nonporous. The adsorbent material is maintained at a temperature below the critical temperature of the adsorbed, 77 K. During adsorption and desorption, the pressure changes until equilibrium is established. To analyse the sample, it is degassed under vacuum for 24 h at room temperature.
In
Figure 3a, the adsorption–desorption isotherm of the composite material, SiO
2Fe
xO
y, is presented, and
Figure 3b shows the pore size distribution obtained using BJH (Barrett, Joyner and Halenda) method from the desorption branch.
Analysing the data obtained and correlating with the IUPAC references [
26], we notice that the analysed material has a specific behaviour to the type IVa isotherm. This type of isotherm has H3-type hysteresis. In this case, capillary condensation occurs faster, but not completely, and the material has pores in the macropore region.
By applying the BJH method for the desorption branch, the pore size distribution shown in
Figure 3b can be obtained. The analysed sample indicates that the material has an average pores size of 12 nm, but, as we can see, macropores are also present (>50 nm).
From the adsorption branch, using the BET method (Brunauer, Emmet, Teller) in the range 0.05–0.3 P/Po, a specific surface of 305 m
2/g is obtained. What is interesting is that the SiO
2Fe
xO
y material, even if it indicates a relatively small specific surface area, has a very large total pore volume, namely 1.55 cm
3/g. The data from the literature show that the pore volume obtained is high, unlike other similar studies [
27,
28], which may lead us to expect good results in terms of vanadium recovery by adsorption on the synthesized material.
3.1.3. Scanning Electron Microscopy (SEM) Analysis
In order to get the adsorbent morphology, the SEM pictures and the EDX spectra were recorded, which prove the predicted composition of newly prepared material (pictures are presented in
Figure 4).
From the image presented in
Figure 4a, it can be observed that the prepared adsorbent materials have a low degree of crystallinity, with several crystals with dimensions between 2 and 20 μm. Moreover, from the EDX spectrum presented in
Figure 4b, we can observe that the prepared material has the expected composition.
3.1.4. Studies on Vanadium Ions Recovery by Adsorption on SiO2FexOy Material
Information regarding the adsorption behaviour of vanadium ions on synthesized xerogels is essential for understanding the mobility of vanadium (V) in aqueous systems. This study investigates the influence of some parameters (S:L ratio, pH, contact time, temperature, and initial concentration of V (V)) on the adsorption capacity of SiO2FexOy material, but also the mechanism of the V adsorption process (V).
3.1.5. Adsorbent Dose Effect on the Adsorption of Vanadium
The effect of solid:liquid (S:L) ratio on the efficiency of the vanadium recovery process is shown in
Figure 5.
It is observed that as the S:L ratio increases, the efficiency of the vanadium adsorption process onto the SiO2FexOy material increases. Starting with the ratio S:L = 0.1 g of adsorbent material:25 mL solution, the efficiency increases, but not significantly (~80%), which determines that all subsequent studies will be carried out at this ratio.
3.1.6. Effect of pH
Vanadium solution pH can affect the adsorption capacity of the prepared adsorptive material, being also studied. Experimental data obtained are presented in
Figure 6.
From data presented in
Figure 6, we can conclude that the highest adsorption capacity was obtained when the adsorption process was conducted at pH = 2 (~8 mg/g) [
29].
Figure 7 shows the Eh–pH diagram presenting the predominant species as a function of pH and redox potential.
Since the pH was set at pH = 2, which is acidic, and the colour of the solutions was yellow, according to
Figure 7, the predominant species is
(E° = 1.0 V) [
30,
31].
3.1.7. Effect of Contact Time and Temperature
The effects of contact time and temperature are shown in
Figure 8.
Data presented in
Figure 8 indicate that with the increase of the contact time, the adsorption capacity of SiO
2Fe
xO
y material increases, up to 90 min. After a period of more than 90 min, the adsorption capacity of the material remains approximately constant (~7.5 mg V (V)/g of adsorbent material), leading us to the conclusion that a contact time of more than 90 min is not required. This behaviour of the adsorbent material can be explained only by considering that the adsorption process is mainly controlled by the inner surface diffusion of vanadium ions (V). Adsorption of vanadium ions from aqueous solution can be considered a long process, until the adsorption equilibrium is reached due to the adsorption of vanadium ions onto the porous material, controlled mainly by an inner surface diffusion process, being much slower than the bulk diffusion [
32].
It is also observed that temperature could positively influence the adsorption capacity of the SiO2FexOy material. Thus, the higher the temperature, the higher the adsorption capacity, such increase being not significant so long as the adsorptive proves being conducted at a temperature of 298 K.
3.1.8. Kinetic Studies
To investigate the kinetics of the vanadium adsorption process on SiO2FexOy, obtained experimental data were modelled using pseudo-first order and pseudo-second order equations.
The kinetics of the studied adsorption process on SiO
2Fe
xO
y adsorbent material were studied at three different temperatures. Thus, in
Figure 9a,b, pseudo-first order and pseudo-second order isotherms are shown.
The adsorption process of V (V) on the studied material proceeds in three stages: (i) a rapid initial stage (the first 40 min), followed by (ii) a slower adsorption stage, and (iii) after 90 min of adsorption to reach balance. The rapid adsorption step can be attributed to easy activation and surface accessibility of the material, but since the sites are covered with V (V) ions, the adsorption rate decreases [
33].
Speed constants values, calculated adsorption capacity values, as well as the values of the regression coefficient, R
2, are presented in
Table 3.
Analysing data presented in
Table 3 can observe that obtained experimental data are well-modelled by the pseudo-second order kinetic model, supported the regression coefficient value close to 1
R2~1 (0.9999–0.9958). By modelling experimental data with the pseudo- first order kinetic model,
R2 values range between 0.9884 and 0.9204. Additionally, data obtained from modelling experimental data with the pseudo-second-order model proved that q
e,calc has values close to q
e,exp. An insignificant influence of temperature on the values of the parameters k
2, q
e,calc, can be observed, so it will be not necessary to work at temperatures higher than 298 K.
3.1.9. Intraparticle Diffusion
The Weber–Morris intraparticle diffusion model was used to further investigate the mechanism of vanadium diffusion on the adsorbent and the controlling steps that affect the adsorption kinetics.
Figure 10 shows the Weber–Morris specific intraparticle diffusion model at 3 temperatures.
Analysing the data presented in
Figure 10, we can observe that the lines obtained from the representation of dependence q
t versus t
1/2 do not pass through origin, signifying that the vanadium adsorption mechanism is a multi-stage one. Based on that, we can conclude that adsorption kinetics is influenced by intraparticle diffusion and by film diffusion. After data modelling, we obtained the values for K
diff and C parameters. Data are presented in
Table 4.
Taking into account data presented in
Table 4, we can observe that, by temperature increase, value of K
diff increases. It is also observed that, for the first stage, diffusion constants are higher than the diffusion constant specific for stage 2, allowing us to conclude that the speed determinant is stage 1, stage 2 being much slower [
34].
Adsorption of vanadium ions from the aqueous phase on the SiO2FexOy adsorbent material can be considered to be a three-stage process: (1) transfer of the sorbent from the aqueous phase to the solid surface, (2) intraparticle diffusion into the pores of the adsorbent, and (3) adsorption at an internal site. Step (3) is assumed to be fast, whereas in terms of (1) and (2) there are steps that can be neglected in any kinetic analysis.
Considering the kinetics of the adsorption process, we can assume that the mass transfer resistance occurs in steps (1) and (2), and can be controlled by acting either individually or in combination. In this study, two kinetic models were presented, namely external mass transfer diffusion and intraparticle mass-transfer diffusion models, to describe the vanadium adsorption mechanism on SiO
2Fe
xO
y [
32,
35].
3.1.10. Activation Energy
The adsorption activation energy V (V) on the SiO
2Fe
xO
y material was evaluated based on the associated equation of the graphical representation ln k
2 = f (1/T) (
Figure 11).
It is observed that the activation energy value (13.7 kJ/mol) is <40 kJ/mol; from this value, we can conclude that the studied adsorption process is a physical one [
31].
3.1.11. Thermodynamic Studies
Thermodynamic studies were performed in the temperature domain between 298 to 318 K.
Figure 12 shows the dependence ln K
d = f (1/T).
Table 5 presents the calculated thermodynamic parameters at all three temperatures.
Upon evaluation of the resulting data, the positive value of ΔH0 means that the adsorption process is endothermic.
It is also observed that ΔG0 has negative values and increases in absolute value with temperature increase, indicating a spontaneous adsorption process, which is influenced by temperature.
The fact that the value of ΔS0 is positive indicates that the adsorption process is favoured, taking place at the interface of the SiO2FexOy material/solution with V (V).
3.1.12. Initial Concentration Effect
The effect of the initial concentration of V
2O
5 on the adsorption capacity of the material is shown in
Figure 13.
From data presented in
Figure 13, we can observe that as the initial concentration of V (V) increases, the adsorption capacity increases. At concentrations greater than 400 mg V (V)/L, the adsorption capacity remains constant (q~58.8 mg V (V)/g), being considered the maximum adsorption capacity of the material.
3.1.13. Equilibrium Studies
Figure 14 presents the adsorption isotherms obtained by the graphical representation of q
e = f (C
e).
Specific parameters associated with each adsorption isotherm used to model obtained experimental data were calculated from slopes of the straight line, and respectively, using the ordinate from the origin (
Table 6).
Data presented in
Figure 14 present the correlation between vanadium equilibrium concentration (C
e) and adsorption capacity, proving that as the equilibrium concentration increases, the adsorption capacity increases until equilibrium is reached, establishing the maximum adsorption capacity obtained experimentally, q
e,exp.
Analysing data presented in
Table 6, we can observe that the studied adsorption process is well-described by the Sips model, as the regression coefficient obtained in this case,
R2, is closest to 1 (
R2 = 0.9914).
The studied adsorption process is homogeneous one. In this case, adsorption occurs through the interaction of a solute molecule with an active centre on the surface of the sorbent. Adsorption occurs on the surface of the sorbent, resulting in a monolayer, the solute molecules being retained only on the free surface of the adsorbent [
32].
A comparison of the adsorption capacity of prepared adsorbent material with the adsorption capacity obtained for some other materials is presented in
Table 7. From presented data, we can observe that the prepared SiO
2Fe
xO
y material has good adsorption capacity.
3.1.14. Desorption Studies
Adsorbent material has been regenerated using two different solutions (NaNO
3 and NaCl) [
31] with a concentration of 5 M. When NaNO
3 5 M was used for regeneration, during the first adsorption/desorption cycle, 75% of adsorbed vanadium ions were desorbed. Further, in the second adsorption/desorption cycle, 67% of adsorbed vanadium was desorbed. In the last adsorption desorption cycle (fourth one), only 38% of adsorbed vanadium was desorbed.
When NaCl was used for the regeneration of the adsorbent material, it was observed that during the first adsorption/desorption cycle, only 57% of adsorbed vanadium had been desorbed. In the third cycle, only 36% of adsorbed vanadium was desorbed, so we can consider that in this case the adsorbent material was exhausted. Based on these observations, we can conclude that the newly prepared adsorbent material can be regenerated using NaNO3 and reused for four times in the vanadium recovery process.
4. Conclusions
The following conclusions can be drawn from the studies presented. In this study, a new material with tuned properties was synthesized, obtaining a composite xerogel based on silica matrices and iron oxides, SiO2FexOy, which proved to be effective for vanadium ions recovery from aqueous solutions by adsorption. Prepared adsorbent material was characterized by X-ray diffraction and N2 sorption analysis.
Vanadium recovery process takes place under the following conditions: S ratio:L = 0.1 g:25 mL, pH = 2, contact time 90 min, and 298 K; studies being performed in batch. Based on obtained results, kinetic, thermodynamic, and equilibrium studies were performed. Kinetically, the pseudo-second order isotherm model is the one that best describes the process.
In order to prove if the determinant step of speed is the film diffusion or the intraparticle diffusion, kinetic experimental data were modelled using the Weber–Morris model. The porous structure of SiO2FexOy material allows the adsorption sites to be placed onto the surfaces located inside the adsorbent channels, which indicates that vanadate can be adsorbed on the surface of SiO2FexOy (stage I), and further reaches equilibrium (stage 2), meaning that intraparticle diffusion is not a speed limiting step during adsorption. Adsorption is performed in films. The activation energy, Ea, was also determined by the fact that the adsorption process is of a physical nature.
Based on thermodynamic studies, we can conclude that the adsorption process is an endothermic, and spontaneous, being influenced by temperature, and that the adsorption process takes place at the interface of the SiO2FexOy material/V (V) solution.
Taking in account performed equilibrium studies, it was observed that the Sips model best describes the adsorption process, establishing that the maximum adsorption capacity of the SiO2FexOy material was 58.8 mg of V ions/g of adsorbent material.
Desorption studies confirm that the adsorption process is controlled by pH, so that if the process proceeds at pH = 2, the material can be recovered and reused with 75% efficiency.
Based on our research, we can conclude that prepared adsorbent material can be used for vanadium recovery from aqueous solutions, with the adsorptive process being endothermic and spontaneous.
Author Contributions
Conceptualization, A.N. and N.D.; Formal analysis, P.N.; Investigation, F.M., M.C., P.I. and C.I.; Writing, A.N. and N.D. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Acknowledgments
This work was supported by a grant of the Romanian Ministry of Research, Innovation and Digitalization, project number PFE 26/30.12.2021, PERFORM-CDI@UPT100. The increasing of the performance of the Polytechnic University of Timișoara by strengthening the research, development, and technological transfer capacity in the field of “Energy, Environment and Climate Change” at the beginning of the second century of its existence, within Program 1—Development of the national system of Research and Development, Subprogram 1.2—Institutional Performance—Institutional Development Projects—Excellence Funding Projects in RDI, PNCDI III”.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Li, M.; Zheng, S.; Liu, B.; Wang, S.; Dreisinger, D.B.; Zhang, Y.; Du, H.; Zhang, Y. A Clean and Efficient Method for Recovery of Vanadium from Vanadium Slag: Nonsalt Roasting and Ammonium Carbonate Leaching Processes. Miner. Processing Extr. Metall. Rev. 2017, 38, 228–237. [Google Scholar] [CrossRef]
- Naumann d’Alnoncourt, R.; Csepei, L.-I.; Hävecker, M.; Girgsdies, F.; Schuster, M.E.; Schlögl, R.; Trunschke, A. The reaction network in propane oxidation over phase-pure MoVTeNb M1 oxide catalysts. J. Catal. 2014, 311, 369–385. [Google Scholar] [CrossRef] [Green Version]
- Amakawa, K.; Kolen’ko, Y.V.; Villa, A.; Schuster, M.E.; Csepei, L.-I.; Weinberg, G.; Wrabetz, S.; Naumann d’Alnoncourt, R.; Girgsdies, F.; Prati, L.; et al. Multifunctionality of Crystalline MoV(TeNb) M1 Oxide Catalysts in Selective Oxidation of Propane and Benzyl Alcohol. ACS Catal. 2013, 3, 1103–1113. [Google Scholar] [CrossRef]
- Hävecker, M.; Wrabetz, S.; Kröhnert, J.; Csepei, L.-I.; Naumann d’Alnoncourt, R.; Kolen’ko, Y.V.; Girgsdies, F.; Schlögl, R.; Trunschke, A. Surface chemistry of phase-pure M1 MoVTeNb oxide during operation in selective oxidation of propane to acrylic acid. J. Catal. 2012, 285, 48–60. [Google Scholar] [CrossRef] [Green Version]
- Slyemi, S.; Barama, A.; Barama, S.; Messaoudi, H.; Casale, S.; Blanchard, J. Comparative study of physico-chemical, acid–base and catalytic properties of vanadium based catalysts in the oxidehydrogenation of n-butane: Effect of the oxide carrier. React. Kinet. Mech. Catal. 2019, 128, 831–845. [Google Scholar] [CrossRef]
- Shcherban, N.D.; Diyuk, E.A.; Sydorchuk, V.V. Synthesis and catalytic activity of vanadium phosphorous oxides systems supported on silicon carbide for the selective oxidation of n-butane to maleic anhydride. React. Kinet. Mech. Catal. 2019, 126, 975–985. [Google Scholar] [CrossRef]
- Liu, J.; Shen, M.; Li, C.; Wang, J.; Wang, J. Enhanced hydrothermal stability of a manganese metavanadate catalyst based on WO3–TiO2 for the selective catalytic reduction of NOx with NH3. React. Kinet. Mech. Catal. 2019, 128, 175–191. [Google Scholar] [CrossRef]
- Perry, S.C.; Pangotra, D.; Vieira, L.; Csepei, L.-I.; Sieber, V.; Wang, L.; Ponce de León, C.; Walsh, F.C. Electrochemical synthesis of hydrogen peroxide from water and oxygen. Nat. Rev. Chem. 2019, 3, 442–458. [Google Scholar] [CrossRef]
- Etcheverry, S.B.; Di Virgilio, A.L.; Barrio, D.A. Vanadium Effects on Bone Metabolism. In Vanadium: Biochemical and Molecular Biological Approaches; Michibata, H., Ed.; Springer: Dordrecht, The Netherlands, 2012; pp. 145–162. [Google Scholar]
- Aureliano, M.; Gumerova, N.I.; Sciortino, G.; Garribba, E.; McLauchlan, C.C.; Rompel, A.; Crans, D.C. Polyoxidovanadates’ interactions with proteins: An overview. Coord. Chem. Rev. 2022, 454, 214344. [Google Scholar] [CrossRef]
- Das, S.; Chatterjee, M.; Janarthan, M.; Ramachandran, H.; Chatterjee, M. Vanadium in Cancer Prevention. In Vanadium: Biochemical and Molecular Biological Approaches; Michibata, H., Ed.; Springer: Dordrecht, The Netherlands, 2012; pp. 163–185. [Google Scholar]
- Ścibior, A.; Pietrzyk, Ł.; Plewa, Z.; Skiba, A. Vanadium: Risks and possible benefits in the light of a comprehensive overview of its pharmacotoxicological mechanisms and multi-applications with a summary of further research trends. J. Trace Elem. Med. Biol. 2020, 61, 126508. [Google Scholar] [CrossRef]
- Mohanty, J.; Rath, P.C.; Bhattacharya, I.N.; Paramguru, R.K. The recovery of vanadium from spent catalyst: A case study. Miner. Processing Extr. Metall. 2011, 120, 56–60. [Google Scholar] [CrossRef]
- Zeng, L.; Yong Cheng, C. A literature review of the recovery of molybdenum and vanadium from spent hydrodesulphurisation catalysts: Part II: Separation and purification. Hydrometallurgy 2009, 98, 10–20. [Google Scholar] [CrossRef]
- Atkins, P.; de Paula, J. Atkins’ Physical Chemistry; Oxford University Press: Oxford, UK, 2005; p. 1008. [Google Scholar]
- Xu, H.; Zhu, S.; Lu, K.; Jia, H.; Xia, M.; Wang, F. Preparation of hierarchically floral ZIF-8 derived carbon@polyaniline@Ni/Al layered double hydroxides composite with outstanding removal phenomenon for saccharin. Chem. Eng. J. 2022, 450, 138127. [Google Scholar] [CrossRef]
- Xu, H.; Zhu, S.; Xia, M.; Wang, F.; Ju, X. Three-dimension hierarchical composite via in-situ growth of Zn/Al layered double hydroxide plates onto polyaniline-wrapped carbon sphere for efficient naproxen removal. J. Hazard. Mater. 2022, 423, 127192. [Google Scholar] [CrossRef]
- Fukunaga, K.; Bhuiyan, M.S. Cardiovascular Protection with Vanadium Compounds. In Vanadium: Biochemical and Molecular Biological Approaches; Michibata, H., Ed.; Springer: Dordrecht, The Netherlands, 2012; pp. 187–207. [Google Scholar]
- Matusoiu, F.; Negrea, A.; Ciopec, M.; Duteanu, N.; Negrea, P.; Svera, P.; Ianasi, C. Molybdate Recovery by Adsorption onto Silica Matrix and Iron Oxide Based Composites. Gels 2022, 8, 125. [Google Scholar] [CrossRef]
- Lagergren, S. About the theory of so-called adsorption of soluble substabces. Kungl. Sven. Vetensk. Handl.-1898 1898, 24, 1–39. [Google Scholar]
- Ho, Y.S. Review of second-order models for adsorption systems. J. Hazard. Mater. 2006, 136, 681–689. [Google Scholar] [CrossRef] [Green Version]
- Weber, W.J.; Morris, J.C. Equilibria and Capacities for Adsorption on Carbon. J. Sanit. Eng. Div. 1964, 90, 79–108. [Google Scholar] [CrossRef]
- Langmuir, I. The adsorption of gases on plane surfaces of glass, mica and platinum. J. Am. Chem. Soc. 1918, 40, 1361–1403. [Google Scholar] [CrossRef] [Green Version]
- Freundlich, H.M.F. Over the adsorption in solution. J. Phys. Chem. 1906, 57, 385–470. [Google Scholar]
- Sips, R. On the Structure of a Catalyst Surface. J. Chem. Phys. 1948, 16, 490–495. [Google Scholar] [CrossRef]
- Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef]
- Ianăşi, C.; Picioruş, M.; Nicola, R.; Ciopec, M.; Negrea, A.; Nižňanský, D.; Len, A.; Almásy, L.; Putz, A.-M. Removal of cadmium from aqueous solutions using inorganic porous nanocomposites. Korean J. Chem. Eng. 2019, 36, 688–700. [Google Scholar] [CrossRef]
- Kondrashova, N.B.; Shamsutdinov, A.S.; Batueva, T.D.; Valtsifer, V.A.; Strelnikov, V.N.; Uporov, S.A. Preparation and Properties of Iron Oxide Doped Mesoporous Silica Systems. J. Inorg. Organomet. Polym. Mater. 2020, 30, 2081–2088. [Google Scholar] [CrossRef]
- Jing, X.; Ning, P.; Cao, H.; Wang, J.; Sun, Z. High-Performance Recovery of Vanadium(V) in Leaching/Aqueous Solution by a Reusable Reagent-Primary Amine N1519. ACS Sustain. Chem. Eng. 2017, 5, 3096–3102. [Google Scholar] [CrossRef]
- Mukherjee, T.K.; Chakraborty, S.P.; Bidaye, A.C.; Gupta, C.K. Recovery of pure vanadium oxide from bayer sludge. Miner. Eng. 1990, 3, 345–353. [Google Scholar] [CrossRef]
- Mthombeni, N.H.; Mbakop, S.; Ochieng, A.; Onyango, M.S. Vanadium (V) adsorption isotherms and kinetics using polypyrrole coated magnetized natural zeolite. J. Taiwan Inst. Chem. Eng. 2016, 66, 172–180. [Google Scholar] [CrossRef]
- Manohar, D.M.; Noeline, B.F.; Anirudhan, T.S. Removal of Vanadium(IV) from Aqueous Solutions by Adsorption Process with Aluminum-Pillared Bentonite. Ind. Eng. Chem. Res. 2005, 44, 6676–6684. [Google Scholar] [CrossRef]
- Zhu, H.; Xiao, X.; Guo, Z.; Han, X.; Liang, Y.; Zhang, Y.; Zhou, C. Adsorption of vanadium (V) on natural kaolinite and montmorillonite: Characteristics and mechanism. Appl. Clay Sci. 2018, 161, 310–316. [Google Scholar] [CrossRef]
- Zhang, S.; Ning, S.; Liu, H.; Zhou, J.; Wang, S.; Zhang, W.; Wang, X.; Wei, Y. Highly-efficient separation and recovery of ruthenium from electroplating wastewater by a mesoporous silica-polymer based adsorbent. Microporous Mesoporous Mater. 2020, 303, 110293. [Google Scholar] [CrossRef]
- McKay, G.; Otterburn, M.S.; Aga, J.A. Fuller’s earth and fired clay as absorbents for dyestuffs external mass transport processes during adsorption. Water Air Soil Pollut. 1985, 26, 149–161. [Google Scholar] [CrossRef]
- Anirudhan, T.S.; Radhakrishnan, P.G. Adsorptive performance of an amine-functionalized poly(hydroxyethylmethacrylate)-grafted tamarind fruit shell for vanadium(V) removal from aqueous solutions. Chem. Eng. J. 2010, 165, 142–150. [Google Scholar] [CrossRef]
- Hu, Q.; Paudyal, H.; Zhao, J.; Huo, F.; Inoue, K.; Liu, H. Adsorptive recovery of vanadium(V) from chromium(VI)-containing effluent by Zr(IV)-loaded orange juice residue. Chem. Eng. J. 2014, 248, 79–88. [Google Scholar] [CrossRef]
- Namasivayam, C.; Sangeetha, D. Removal and recovery of vanadium(V) by adsorption onto ZnCl2 activated carbon: Kinetics and isotherms. Adsorption 2006, 12, 103–117. [Google Scholar] [CrossRef]
- Naeem, A.; Westerhoff, P.; Mustafa, S. Vanadium removal by metal (hydr)oxide adsorbents. Water Res. 2007, 41, 1596–1602. [Google Scholar] [CrossRef]
Figure 1.
SiO2FexOy xerogel synthesis scheme.
Figure 1.
SiO2FexOy xerogel synthesis scheme.
Figure 2.
X-ray diffraction.
Figure 2.
X-ray diffraction.
Figure 3.
N2 adsorption-desorption isotherm for composite material (a) and pore size distribution (b).
Figure 3.
N2 adsorption-desorption isotherm for composite material (a) and pore size distribution (b).
Figure 4.
SEM picture recorded for prepared adsorbent material (a) and EDX spectra obtained for prepared adsorbent material (b).
Figure 4.
SEM picture recorded for prepared adsorbent material (a) and EDX spectra obtained for prepared adsorbent material (b).
Figure 5.
Effect of the dose of adsorbent on vanadium ions adsorption on the SiO2FexOy material.
Figure 5.
Effect of the dose of adsorbent on vanadium ions adsorption on the SiO2FexOy material.
Figure 6.
Effect of pH on the adsorption mount of vanadium (V).
Figure 6.
Effect of pH on the adsorption mount of vanadium (V).
Figure 7.
Relationship between the state of vanadium in aqueous solution and vanadium concentration and pH [
30].
Figure 7.
Relationship between the state of vanadium in aqueous solution and vanadium concentration and pH [
30].
Figure 8.
Effect of contact time and temperature on the V(V) recovery.
Figure 8.
Effect of contact time and temperature on the V(V) recovery.
Figure 9.
Pseudo-first order (a) and pseudo-second order isotherms (b).
Figure 9.
Pseudo-first order (a) and pseudo-second order isotherms (b).
Figure 10.
Intraparticle diffusion models for three different temperatures.
Figure 10.
Intraparticle diffusion models for three different temperatures.
Figure 11.
Ln k2 vs. 1/T plot for SiO2FexOy material.
Figure 11.
Ln k2 vs. 1/T plot for SiO2FexOy material.
Figure 12.
Thermodynamic studies for determination of ln Kd vs. 1/T plot for SiO2FexOy sample.
Figure 12.
Thermodynamic studies for determination of ln Kd vs. 1/T plot for SiO2FexOy sample.
Figure 13.
Effect of initial concentration on the adsorption capacity for SiO2FexOy sample.
Figure 13.
Effect of initial concentration on the adsorption capacity for SiO2FexOy sample.
Figure 14.
Equilibrium isotherms for SiO2FexOy sample.
Figure 14.
Equilibrium isotherms for SiO2FexOy sample.
Table 1.
Kinetic equations.
Table 1.
Kinetic equations.
Model | Equation | Reference |
---|
Pseudo-first order model (Lagergren model) | where: qe—equilibrium adsorption capacity, mg/g qt—adsorption capacity at t time, mg/g k1—speed constant for pseudo-first order equation, 1/min t—contact time, min. | [20] |
Pseudo-second order model (Ho și McKay model) | where: qe—equilibrium adsorption capacity, mg/g qt—adsorption capacity at t time, mg/g k2—speed constant for pseudo-second order equation, g/mg∙min t—contact time, min. | [21] |
Intraparticle diffusion (Weber and Morris model) | qt = kdiff · t1/2 + C where: qt—adsorption capacity at t time, mg/g kdiff—speed constant for intraparticle diffusion, mg/g·min1/2 C—constant correlated with the thickness of the liquid film surrounding the adsorbent particles. | [22] |
Table 2.
Equilibrium isotherms.
Table 2.
Equilibrium isotherms.
Isotherms Model | Equation | Reference |
---|
Nonlinear Langmuir isotherm | where: qL—Langmuir maximum adsorption capacity, mg/g KL—Langmuir constant Ce—equilibrium concentration, mg/L Qe—equilibrium adsorption capacity, mg/g | [23] |
Linear Langmuir isotherm | where: qL—Langmuir maximum adsorption capacity, mg/g KL—Langmuir constant Ce—equilibrium concentration, mg/L Qe—equilibrium adsorption capacity, mg/g | [23] |
Nonlinear Freundlich isotherm | where: KF and nF—characteristic constants that may be related to the relative adsorption capacity of the adsorbent and the adsorption intensity Ce—equilibrium concentration, mg/L | [24] |
Linear Freundlich isotherm | where: KF and nF—characteristic constants that may be related to the relative adsorption capacity of the adsorbent and the adsorption intensity Ce—equilibrium concentration, mg/L | [24] |
Nonlinear Sips isotherm | where: KS—constant related to the adsorption capacity of the adsorbent, nS—heterogeneity factor Ce—equilibrium concentration, mg/L | [25] |
Table 3.
Kinetic parameters.
Table 3.
Kinetic parameters.
Pseudo-First Order |
Temperature (K) | qe,exp(mg/g) | k1(min−1) | qe,calc(mg/g) | R2 |
298 | 7.18 | 0.0108 | 4.10 | 0.9884 |
308 | 7.45 | 0.0185 | 6.54 | 0.9694 |
318 | 7.48 | 0.0201 | 7.18 | 0.9204 |
Pseudo-Second Order |
Temperature (K) | qe,exp(mg/g) | k2(g/mg∙min) | qe,calc(mg/g) | R2 |
298 | 7.18 | 5.93 | 7.24 | 0.9999 |
308 | 7.45 | 6.98 | 7.40 | 0.9983 |
318 | 7.48 | 8.40 | 7.69 | 0.9958 |
Table 4.
Specific parameters of intraparticle diffusion for SiO2FexOy.
Table 4.
Specific parameters of intraparticle diffusion for SiO2FexOy.
Intraparticle Diffusion Model |
---|
Temperature (K) | Kdiff (mg/g·min1/2) | C | R2 |
---|
298 | 0.27 | 2.57 | 0.8539 |
308 | 0.31 | 3.80 | 0.8543 |
318 | 0.37 | 4.26 | 0.8169 |
Table 5.
Thermodynamic parameters.
Table 5.
Thermodynamic parameters.
ΔH0, kJ/mol | ΔS0, J/mol∙K | ΔG0 kJ/mol | R2 |
---|
19.76 | 82.28 | 298 K | 308 K | 318 K | 0.9985 |
−4.75 | −5.57 | −6.40 |
Table 6.
Isotherm parameters.
Table 6.
Isotherm parameters.
Langmuir Isotherm |
qm,exp (mg/g) | KL (L/mg) | qL (mg/g) | R2 |
58.75 | 0.0064 | 93.95 | 0.9120 |
Freundlich Isotherm |
KF (mg/g) | 1/nF | R2 |
2.35 | 0.57 | 0.8347 |
Sips Isotherm |
KS | qS (mg/g) | 1/nS | R2 |
2.8·10−5 | 61.0 | 1.4 | 0.9914 |
Table 7.
Adsorption performance comparison.
Table 7.
Adsorption performance comparison.
Materials | q, mg/g | References |
---|
montmorillonite | 0.98 | [33] |
kaolinite | 0.78 | [33] |
Aluminum-pillared Bentonite, Al-PILC | 24.16 | [32] |
FeOOH | 45.6 | [31] |
PGTFS-NH3+Cl− | 45.86 | [36] |
Zr(IV)–SOW | 56.75 | [37] |
ZnCl2 activated carbon | 24.9 | [38] |
Metal hydroxide adsorbents: TiO2 | 25.06 | [39] |
SiO2FexOy | 58.8 | This study |
| Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations. |