Next Article in Journal
Ultra-High Strength in FCC+BCC High-Entropy Alloy via Different Gradual Morphology
Previous Article in Journal
Predicting High-Strength Concrete’s Compressive Strength: A Comparative Study of Artificial Neural Networks, Adaptive Neuro-Fuzzy Inference System, and Response Surface Methodology
Previous Article in Special Issue
Using the IL-TEM Technique to Understand the Mechanism and Improve the Durability of Platinum Cathode Catalysts for Proton-Exchange Membrane Fuel Cells
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Corrosion Behaviour of Weld Metal of Ultra-High-Strength Steel Weldments in a Sodium Chloride Aqueous Solution

Department of Materials Science and Technology, University of Ruse “Angel Kanchev”, 8 Studentska St., 7017 Ruse, Bulgaria
*
Author to whom correspondence should be addressed.
Materials 2024, 17(18), 4534; https://doi.org/10.3390/ma17184534
Submission received: 30 July 2024 / Revised: 20 August 2024 / Accepted: 12 September 2024 / Published: 15 September 2024

Abstract

:
As high-strength and ultra-high-strength steels are widely used in all kinds of modern welded constructions, a lot of research is carried out to investigate the mechanical properties of the weldments of these steels, but there is little information on such important characteristics as their corrosion behaviour. This research focuses on the corrosion behaviour of the weld metal of the weldments of S906QL and S700MC steels. The weld metal was tested electrochemically in a 3.5% NaCl aqueous solution via a potentiodynamic scan to determine the corrosion rate and its dependence on the welding gap. No influence of the welding gap on the corrosion rate was found, but the experimental results suggested that the corrosion rate depended on the chemical composition of the filler material and the microstructure of the weld metal.

1. Introduction

The need for energy savings and environmental preservation has led to the development of high-strength steels. Structural steels with a high yield point are known as high-strength steels (HSSs), and when the yield point of the steels is above 700 MPa, they are called ultra-high-strength steels (UHSSs) [1]. Both HSS and UHSS have various practical uses, ranging from construction to automotive and spacecraft production. In the modern world, HSS and UHSS play a key role in global warming, as these steels offer high strength combined with reduced vehicle weight and different structures, thus lowering harmful emissions. For instance, lighter trucks made of high-strength steel can carry more goods while emitting the same amount of CO2 per kilometre [2]. As HSS and UHSS offer the same or increased strength at reduced weight compared to conventional steels, their use allows more energy-efficient and cost-efficient designs for vehicles, wind turbines, transformers, motors, and other types of construction. This leads to a reduction in energy consumption throughout the lifespan of the equipment and construction. Therefore, HSS and UHSS enhance structural performance and also support environmental preservation by reducing emissions and promoting sustainable practices.
High-strength steels obtain their mechanical properties after careful steel composition design and heat treatment or thermo-mechanical treatment. An example of heat-treated ultra-high-strength steel is S960QL. S960QL has a high yield strength (up to 960 MPa depending on the thickness) due to the combination of the proper choice of alloying elements and heat treatment—quenching and tempering. S700MC is another example of ultra-high-strength steel. The high yield strength of S700MC (700 MPa) is achieved by a combination of microalloying and thermo-mechanical treatment, i.e., rolling at elevated temperatures and then accelerated cooling.
Both grades possess good weldability; therefore, S960QL and S700MC weldments are widely used in different welded structures. Numerous studies have been conducted on the structure and mechanical properties of S960QL and S700MC weldments [3,4,5,6,7,8,9,10,11,12,13,14,15]. Unfortunately, information on the corrosion behaviour of the weldments of both steels is hard to find in the specialised literature. It is well known that different zones in the weldments and base metal demonstrate different corrosion rates, and this leads to the formation of corrosion galvanic elements. Nevertheless, a more detailed exploration work on the corrosion behaviour of weldments is needed to assess the lifespan of welded structures and the most probable spots for corrosion to occur to prevent the loss of mechanical stability and structural integrity.
The present paper focuses on the determination of the corrosion rates of the weld metal (fusion zone) of the weldments of S960QL and S700MC in the most abundant electrolyte on our planet, i.e., the sodium chloride water solution, using accelerated electrochemical testing. As the use of a standardised weld gap is not suitable in various applications, the weldments tested here were made with different welding gaps, and the influence of the welding gaps on the corrosion of weld metal was experimentally found.

2. Materials and Methods

The tested specimens were weldments of S960QL and S700MC. The detailed welding procedures are described in [16,17]. Both steels were manufactured by Voestalpine Stahl GmbH (Linz, Austria). S960QL came as a plate with a thickness of 6 mm, and S700MC came as hot-rolled sheets with a thickness of 8 mm. The chemical composition of the steels, according to the manufacturer, is given in Table 1.
The welded parts had dimensions of 500 × 150 × 6 mm for S960QL and 500 × 150 × 8 mm for S700MC (length, width, thickness), following ISO 15614-1:2017 [18]. As the welding method, submerged arc welding was used, with direct current and reverse polarity DC (+). Four different welding gaps of 0 mm, 4 mm, 6 mm, and 8 mm were used as described in [16,17]. Except for the welding gap root, which had to be investigated for its impact on the weldments, the joint preparation followed ISO 9692-2:2001 [19]. Without a root face, a mechanical bevel was performed at an angle of 30° (for a total of 60°). As a filler material, a wire of AWS ER120S-G for S960QL was used, and for S700MC, a wire of AWS ER 100S-G was used, manufactured by ESAB (North Bethesda, MD, USA). In both cases, the diameter of the filler material was 1.2 mm, and the flux was S A AB 1 56 AC H5 (ISO 14174:2019 [20]). The chemical composition of the filler materials, according to the manufacturer, is shown in Table 2, and the welding parameters are shown in Table 3.
Test specimens of the weldments were cut off after welding to examine the macrostructure and microstructure and to perform corrosion tests. The macrostructure was examined in two directions—parallel to the welding direction and normal to the welding direction. Prior to etching for macrostructural analysis, the specimens were wet ground with 240, 320, 400, 500, 600, 800, and 1000 SiC grit. For macrostructure evaluation, a saturated FeCl3 (ITW Reagents, Barcelona, Spain) water solution was used at room temperature for 15 s. Metallographic examination was performed on the microsections normal to the welding direction after wet grinding and mechanical polishing with Al2O3 0.5 µm (Leco, St. Joseph, MI, USA) and final polishing with Al2O3 0.03 µm (Leco, St. Joseph, MI, USA). A 3% HNO3 (ITW Reagents, Barcelona, Spain) alcohol solution was used for etching the microsections for 5 s. An optical Epitip 2 (Carl Zeiss Jena, Jena, Germany) microscope equipped with a digital camera was used to observe the microstructure and to take microphotographs of it. In the Results Section, only a few representative microphotographs are given.
The corrosion rate was evaluated using accelerated electrochemical testing. Electrochemical tests were carried out on the weld metal surface, parallel to the welding direction, as shown in Figure 1. The tested surfaces were ground and polished for metallographic examination and cleaned with acetone. As an aggressive environment, a neutral 3.5% NaCl (ITW Reagents, Barcelona, Spain) water solution was chosen as this is the average sodium chloride concentration in the world’s oceans [21]. Prior to the electrochemical test, every specimen was allowed to stabilise in the electrolyte for 50 min. At the end of this stabilisation period, the steady state potential Ess was measured against a saturated calomel electrode SCE. The potential of the SCE at the test room temperature (the temperature of the solution was 19 °C) was +245 mV against the standard hydrogen electrode SHE, and all the values of the potentials presented here are calculated according to this value against the SHE. Following this was linear polarisation using a standard three-electrode cell with the tested sample as a working electrode, the SCE as a reference electrode, and a Pt-counter electrode. The potential was controlled using a Radelkis OH 105 (Radelkis, Budapest, Hungary) potentiostat equipped with a National Instruments USB-6008 controller (National Instruments, Austin, TX, USA) connected to a computer. The area of the tested surfaces was 0.5 cm2, and the rate of potential increase was 1 mV/s, starting from −650 mV up to −250 mV. eL-ChemViewer software, version 3.3 [22] was used for Tafel analysis for corrosion current density icorr and corrosion potential Ecorr determination. Using the obtained icorr values, the corrosion penetration rate CR was calculated, as described in [23]. To assure experimental reliability, three specimens of every welding mode, as well as of the two base metals, were tested. Here, the averaged values are presented.

3. Results

The present work aims to characterise the weld metal. First, to evaluate the corrosion behaviour of the weld metal, macrostructural analysis of the weld metal of the weldments was performed. Figure 1 presents the macrostructure of the surfaces of some of the tested weldments. The weld metal (WM) on the longitudinal sections of both steels looks similar, except for the visible isotherms on the S960QL weld metal—curved lines, showing how the pool moved during welding. Near the WM boundaries, curved dendrites are observed for both steels’ weldments, and approaching the centre line of the weldments, the shape of the WM changes to an equiaxed one.
To find the faults and depth of fusion, cross-sections of the samples of both steels were observed, as shown in Figure 2 and Figure 3.
For all the welding modes, faults are not observed, but the weldments show full penetration. With the increase in the weld gap dimension, the width of the sum of the different welding zones increases too, as was expected. It is interesting to note that the coarse-grained heat-affected zone on the weldments of S700MC is narrower than the observed one on the weldments of S960QL. The weld metal of all the weldments demonstrates a typical dendritic (cast) structure with grains elongated towards the weld root near the weld centre line and toward the heat-affected zone near the ends of the WM. Increasing the distance between the welded parts leads to an increase in the weld’s asymmetry. A detailed description of the macrostructure of the weldments studied here is given in [16,17].
The microstructure of the specimens of S960QL is presented in Figure 4, and the microstructure of the specimens made of S700MC is given in Figure 5. The S960QL steel demonstrates a homogeneous-looking microstructure, consisting of tempered martensite and bainite—Figure 4a,b. The microstructure of the S700MC steel is composed of ferrite and bainite [17] and shows signs of the thermo-mechanical treatment the steel was subjected to by the manufacturer—Figure 5a,b. The microstructure of the weld metals of all the weldments demonstrates a cast structure with a white constituent as elongated grains—Figure 4 and Figure 5. This white constituent is ferrite and is larger in terms of share and dimensions in the WM of the S700MC than in the WM of the S960QL weldments, as is visible in Figure 4 and Figure 5.
The tested surfaces are shown in Figure 1. As the opening of the specimens’ holder for corrosion testing was 8 mm and the specimens were centred in the holder, the results presented here only give information about the corrosion behaviour of the weld metal near the centre line of the weldments.
The open circuit potential OCP and its change in time are shown in Figure 6 for the S960QL specimens and in Figure 7 for the S700MC specimens. The values of steady state potential Ess are summarised in Table 3. While S960QL demonstrates more negative OCP and Ess than the weld metal of the weldments of S960QL, S700MC displays a more noble potential than its weldments.
Figure 8 shows the results from the potentiodynamic scan of the specimens of S960QL, and Figure 9 shows those of the S700MC specimens. Corrosion potential Ecorr, corrosion current density icorr, and calculated corrosion penetration rate CR are presented in Table 3. It is seen in Figure 8 that the weld gap does not categorically influence the corrosion potential of WM on S960QL—the weld metal of the weldments made by welding modes W1 and W2 has slightly more positive values of Ecorr, while the corrosion potential values of the weld metal of the weldments obtained by welding modes W3 and W4 are shifted in a negative direction. Nevertheless, regarding corrosion current density, the corrosion rates of the weld metal of all the weldments of S960QL are lower by one order of magnitude than those of the base metal. A different picture is observed for the specimens made of S700MC—the corrosion potential of the weld metal of all the specimens of S700MC is shifted towards more negative values compared to the base metal, and the corrosion current density and corrosion rate outweigh the corresponding values for the base metal by one order of magnitude. No local corrosion damage was observed after electrochemical testing, but uniform surface dissolution was seen.

4. Discussion

The corrosion behaviour of the weld metal of the weldments studied here should be governed by their structure and the specific corrosion medium. The difference in chemical composition between the base metal and weld metal must also be taken into account when discussing practical implications.
The role of the medium. The formation of thick stable protective passive layers for both steels in the used neutral solution or in air is not possible; so, the tested surfaces are unprotected from the action of aggressive ions. As the sodium chloride concentration in the solution is low, oxygen solubility is at its highest levels, and there is enough dissolved oxygen to reach the cathodic areas on the specimens’ surfaces and for the corrosion process to take place without an effective diffusion—a barrier film to prevent the anodic dissolution of the specimens [24]. Thus, one can expect that the main factors controlling the dissolution of the specimens are their structure and chemical composition.
The role of structure and chemical composition. As described in [25], the addition of Ni to a medium-carbon ultra-high-strength steel leads to a decrease in the corrosion rate. This effect is profound up to 0.5 wt.% Ni, and the next increase up to 1 wt.% in Ni content only slightly decreases the corrosion rate, but the open circuit potential increases consistently with Ni addition to an acid medium. The beneficial effect of Ni on the corrosion rate of medium-carbon steel in a neutral NaCl aqueous solution is attributed to the formation of a thin, rich Ni layer under the outer layer of iron oxides [25].
S960QL and S700MC both have a bainite constituent, but the S700MC base metal also reveals an equilibrium constituent—ferrite grains—while the microstructure of the S960QL base metal is an entirely non-equilibrium microstructure: tempered martensite and bainite. Despite the higher concentration of Ni and Cu in S960QL, this non-equilibrium microstructure and the micro-stresses connected to it led to the higher corrosion rate of S9600QL compared to the S700MC base metal.
The weld metal was characterised by a dendritic structure, but due to the directional crystallisation, opposite to the heat output, the grains on all tested surfaces of the weld metal showed an almost equiaxed shape. The microstructure of the weld metal of the S700MC specimens was characterised by a larger amount of idiomorphic ferrite. According to [26], idiomorphic ferrite in weld metal forms when non-metallic inclusions, mostly oxides, serving as nucleation sites for the heterogeneous nucleation of ferrite, are present in the weld metal. This indicates that oxygen in a larger amount entered the weld pool during welding. The presence of idiomorphic ferrite was more pronounced for the weldments of S700MC obtained by welding modes W3 and W4, but it did not affect the corrosion behaviour of the weld metal, as is visible in Figure 7 and Figure 9 and Table 4.
The Ni concentration in S960QL was 0.039 wt.%, and in the filler metal, it was 2.22 wt.%, i.e., more than 56 times higher. The real cooling rates during welding did not allow a significant diffusion of Ni atoms toward the base metal, thus leaving the nickel concentration as the highest in the weld metal. During the non-equilibrium phase transformation following crystallisation, most of Ni atoms remained locked in martensite and retained austenite, and some of them remained in the newly formed ferrite. As the weldments were not subjected to heat treatment, the structural stresses in the weld metal were higher than those in the base metal. Thus, the corrosion behaviour of the weld metal of the weldments of S960QL was a result of two opposing phenomena: (1) A local enrichment of weld metal in Ni, decreasing the corrosion rate and (2) a high level of structural stresses, increasing the corrosion rate. As is visible in Figure 6 and Figure 8 and Table 4, none of these phenomena prevails when only OCP, Ess, and Ecorr are considered, but obviously, the above-mentioned richness in the Ni layer led to some protection of the weld metal, and the corrosion rate decreased.
The weld metal of the weldments of S700MC showed worsening corrosion behaviour compared to the base metal. Apparently, the chemical composition of the filler material did not work to keep the corrosion potential and steady state potential unchanged. The electrochemical reaction on the weld metal’s surface occurred with cathodic control as the steady state and corrosion potentials of the weld metal were close to the standard electrode potential of pure iron. Nevertheless, both the anodic and cathodic current densities of the weld metal of the S700MC specimens were higher than those of the base metal. Thus, the non-equilibrium microstructure of the weld metal was the factor which controlled the corrosion behaviour of the weld metal of the S700MC samples, and it resulted in greater the corrosion rates of the weld metal.
For the weld metal of all the weldments of both steels, the welding gap did not affect the corrosion behaviour.
As the steady state and corrosion potentials of the weld metal of all the weldments of S700MC were shifted in a negative direction, the appearance of a corrosion galvanic cell could be expected with the weld metal acting as an anode and the base metal acting as a cathode. Since the potential difference between the base metal and weld metal is not so pronounced (40 to 50 mV), the resulting current should not have high values. Nevertheless, the base metal surpasses the weld metal in area, i.e., the base metal represents a cathode consuming a considerable number of electrons. Thus, in real working environments that promote corrosion processes, a high corrosion rate and dissolution of the weld metal is to be expected.
The appearance of a corrosion galvanic cell is also expected for the specimens of S960QL, but in this case, the role of the anode and cathode could not be categorically specified. Despite this, preventive measures should be considered when employing weldments of S960QL and S700MC, and the practical one is corrosion protection painting.

5. Conclusions

The results presented in this work focus on the corrosion behaviour of weld metal. The weldments consist of more zones than a weld metal and to completely characterise them future research must be conducted; however, the experiments presented here add to the scarce information about the corrosion behaviour of the weldments of high-strength steels.
The practical conclusion about the influence of the width of the welding gap on the corrosion behaviour of weld metal is that when designing welding modes no consideration with respect to corrosion is needed, as the width of the welding gap does not affect the corrosion behaviour of the weld metal of the weldments of S960QL and S700MC in 3.5% NaCl aqueous solution.
The corrosion behaviour of the weld metal depends on its microstructure and the chemical composition of the filler materials, and neither of these two factors always prevails. Thus, the filler material for the welding of S960QL leads to a decrease in the corrosion rate of the weld metal despite its non-equilibrium microstructure, but the corrosion behaviour of the weld metal of the weldments of S700MC is governed by its non-equilibrium microstructure, and the filler material does not affect it in 3.5% NaCl aqueous solution.
For practical purposes, corrosion prevention of the weldments of S960QL and S700MC with paints is recommended.

Author Contributions

Conceptualisation, M.I., N.F. and R.R.; methodology, M.I., N.F. and R.R.; microstructural analysis, M.I. and D.G.; corrosion analysis, M.I.; investigation, M.I. and D.G.; software, M.I.; validation, M.I. and R.R.; resources, N.F., D.G. and R.R.; writing—original draft preparation, M.I.; writing—review and editing, M.I. and D.G.; visualisation, M.I. All authors have read and agreed to the published version of the manuscript.

Funding

This study is financed by the European Union-NextGenerationEU, through the National Recovery and Resilience Plan of the Republic of Bulgaria, project № BG-RRP-2.013-0001-C01.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The original contributions presented in the study are included in the article, further inquiries can be directed to the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Tümer, M.; Schneider-Bröskamp, C.; Enzinger, N. Fusion welding of ultra-high strength structural steels—A review. J. Manuf. Process. 2022, 82, 203–229. [Google Scholar] [CrossRef]
  2. World Steel Association. Steel’s Contribution to a Low Carbon Future and Climate Resilient Societies—World Steel Position Paper; World Steel Association: Brussels, Belgium, 2019; ISBN 978-2-930069-83-8. Available online: https://canadiansteel.ca/files/resources/Position_paper_climate_2019_vfinal.pdf (accessed on 1 July 2024).
  3. Sisodia, R.P.; Gáspár, M. Experimental assessment of microstructure and mechanical properties of electron beam welded S960M high strength structural steel. Manuf. Lett. 2021, 29, 108–112. [Google Scholar] [CrossRef]
  4. Zhang, L.; Kannengiesser, T. Austenite grain growth and microstructure control in simulated heat affected zones of microalloyed HSLA steel. Mater. Sci. Eng. A 2014, 613, 326–335. [Google Scholar] [CrossRef]
  5. Sun, J.; Dilger, K. Influence of preheating on residual stresses in ultra-high strength steel welded components. J. Mater. Res. Technol. 2023, 25, 3120–3136. [Google Scholar] [CrossRef]
  6. Gorka, J.; Kotarska, A. MAG welding of 960QL quenched and tempered steel. In IOP Conference Series: Materials Science and Engineering 591, Modern Technologies in Industrial Engineering VII (ModTech2019), Iasi, Romania, 19–22 June 2019; IOP Publishing: Bristol, UK, 2019. [Google Scholar]
  7. Türker, M. The Effect of Welding Parameters on Microstructural and Mechanical Properties of HSLA S960QL Type Steel with Submerged Arc Welding. J. Nat. Appl. Sci. 2017, 21, 673–682. [Google Scholar] [CrossRef]
  8. Szymczak, T.; Szczucka-Lasota, B.; Węgrzyn, T.; Łazarz, B.; Jurek, A. Behavior of Weld to S960MC High Strength Steel from Joining Process at Micro-Jet Cooling with Critical Parameters under Static and Fatigue Loading. Materials 2021, 14, 2707. [Google Scholar] [CrossRef] [PubMed]
  9. Garašić, I.; Ćorić, A.; Kožuh, Z.; Samardzic, I. Occurrence of cold cracks in welding of high-strength S960 QL steel. Teh. Vjesn.-Tech. Gaz. 2010, 17, 327–335. [Google Scholar]
  10. Sisodia, R.P.S.; Gáspár, M. An Approach to Assessing S960QL Steel Welded Joints Using EBW and GMAW. Metals 2022, 12, 678. [Google Scholar] [CrossRef]
  11. Ślęzak, T. Fatigue Examination of HSLA Steel with Yield Strength of 960 MPa and Its Welded Joints under Strain Mode. Metals 2020, 10, 228. [Google Scholar] [CrossRef]
  12. Guo, W.; Crowther, D.; Francis, J.A.; Thompson, A.; Liu, Z.; Li, L. Microstructure and mechanical properties of laser welded S960 high. Mater. Des. 2015, 85, 534–548. [Google Scholar] [CrossRef]
  13. Kik, T.; Górka, J.; Kotarska, A.; Poloczek, T. Numerical Verification of Tests on the Influence of the Imposed Thermal Cycles on the Structure and Properties of the S700MC Heat-Affected Zone. Metals 2020, 10, 974. [Google Scholar] [CrossRef]
  14. Moravec, J.; Sobotka, J.; Novakova, I.; Bukovska, S. Assessment the Partial Welding Influences on Fatigue Life of S700MC Steel Fillet Welds. Metals 2021, 11, 334. [Google Scholar] [CrossRef]
  15. Skowrońska, B.; Chmielewski, T.; Golański, D.; Szulc, J. Weldability of S700MC steel welded with the hybrid plasma + MAG method. Manuf. Rev. 2020, 7, 4. [Google Scholar] [CrossRef]
  16. Ferdinandov, N.; Gospodinov, D.; Ilieva, M.; Radev, R. Structure and Mechanical Properties of High Strength Steel 960QL Weldments. Defect Diffus. Forum 2022, 416, 93–101. [Google Scholar] [CrossRef]
  17. Ferdinandov, N.; Gospodinov, D.; Ilieva, M.; Radev, R. Effect of the Root Gap on the Structure and Properties of High Strength Steel S700MC Welds. Key Eng. Mater. 2021, 890, 201–208. [Google Scholar] [CrossRef]
  18. BIS EN ISO 15614-1:2017; Specification and Qualification of Welding Procedures for Metallic Materials—Welding Procedure Test—Part 1: Arc and Gas Welding of Steels and Arc Welding of Nickel and Nickel Alloys (ISO 15614-1:2017, Corrected Version 2017-10-01). Bulgarian Institute for Standardization: Sofia, Bulgaria, 2017.
  19. BIS EN ISO 9692-2:2001; Welding and Allied Processes—Joint Preparation—Part 2: Submerged Arc Welding of Steels (ISO 9692-2:2001). Bulgarian Institute for Standardization: Sofia, Bulgaria, 2001.
  20. BIS EN ISO 14174:2019; Welding Consumables—Fluxes for Submerged Arc Welding and Electroslag Welding—Classification (ISO 14174:2019). Bulgarian Institute for Standardization: Sofia, Bulgaria, 2019.
  21. Salinity. Available online: https://salinity.oceansciences.org/overview.htm#:~:text=On%20average%2C%20sea%20surface%20salinity,and%20ice%20freezing%20and%20melting (accessed on 1 July 2024).
  22. Hrbac, J.; Halouzka, V.; Trnkova, L.; Vacek, J. eL-Chem Viewer: A Freeware Package for the Analysis of Electroanalytical Data and Their Post-Acquisition Processing. Sensors 2014, 14, 13943–13954. [Google Scholar] [CrossRef] [PubMed]
  23. ASTM G102-89; Standard Practice for Calculation of Corrosion Rates and Related Information from Electrochemical Measurements. ASTM International: West Conshohocken, PA, USA, 2015.
  24. Revie, R.W.; Uhlig, H.H. Corrosion and Corrosion Control: An Introduction to Corrosion Science and Engineering, 4th ed.; John Wiley & Sons, Inc.: Hoboken, NJ, USA, 2008. [Google Scholar]
  25. Mohrbacher, H.; Kern, A. Nickel Alloying in Carbon Steel: Fundamentals and Applications. Alloys 2023, 2, 1–28. [Google Scholar] [CrossRef]
  26. Liu, S.; Indacochea, J.E. Control of chemical composition and microstructure in low carbon microalloyed steel weldments. In Welding: Theory and Practice; Olson, D.L., Dixon, R., Liby, A., Eds.; Elsevier Science Publishers B.V.: Amsterdam, The Netherlands, 1990; Volume 8, pp. 118–148. [Google Scholar]
Figure 1. Macrostructure of the weldments, longitudinal section.
Figure 1. Macrostructure of the weldments, longitudinal section.
Materials 17 04534 g001
Figure 2. Macrostructure of weldments of S960QL, cross-section.
Figure 2. Macrostructure of weldments of S960QL, cross-section.
Materials 17 04534 g002
Figure 3. Macrostructure of weldments of S700MC, cross-section.
Figure 3. Macrostructure of weldments of S700MC, cross-section.
Materials 17 04534 g003
Figure 4. Microstructure of the base metal (BM) and weld metal (WM) of the weldments of S960QL at two different magnifications.
Figure 4. Microstructure of the base metal (BM) and weld metal (WM) of the weldments of S960QL at two different magnifications.
Materials 17 04534 g004aMaterials 17 04534 g004b
Figure 5. Microstructure of the base metal (BM) and weld metal (WM) of the weldments of S700MC at two different magnifications.
Figure 5. Microstructure of the base metal (BM) and weld metal (WM) of the weldments of S700MC at two different magnifications.
Materials 17 04534 g005aMaterials 17 04534 g005b
Figure 6. Open circuit potential of S960QL and weld metal of weldments of S960QL in a 3.5% NaCl water solution at room temperature.
Figure 6. Open circuit potential of S960QL and weld metal of weldments of S960QL in a 3.5% NaCl water solution at room temperature.
Materials 17 04534 g006
Figure 7. Open circuit potential of S700MC and weld metal of weldments of S700MC in a 3.5% NaCl water solution at room temperature.
Figure 7. Open circuit potential of S700MC and weld metal of weldments of S700MC in a 3.5% NaCl water solution at room temperature.
Materials 17 04534 g007
Figure 8. Polarisation curves of S960QL and weld metal of weldments of S960QL in a 3.5% NaCl water solution at room temperature.
Figure 8. Polarisation curves of S960QL and weld metal of weldments of S960QL in a 3.5% NaCl water solution at room temperature.
Materials 17 04534 g008
Figure 9. Polarisation curves of S700MC and weld metal of weldments of S700MC in a 3.5% NaCl water solution at room temperature.
Figure 9. Polarisation curves of S700MC and weld metal of weldments of S700MC in a 3.5% NaCl water solution at room temperature.
Materials 17 04534 g009
Table 1. Chemical composition of S960QL and S700MC steels.
Table 1. Chemical composition of S960QL and S700MC steels.
Chemical Composition of S960QL in Weight %
CSiMnPSAlBCrCuMoNNbNiTiVZr
0.1750.2491.0750.0090.0010.0840.00230.6200.0180.6080.00390.0290.0390.0030.0020.001
Chemical Composition of S700MC in Weight %
CSiMnPSAlBCrCuMoNNbNiTiVZr
0.0650.0491.8300.0060.00060.0510.00020.0250.0090.002-0.0490.0090.1230.008-
Table 2. Chemical composition of AWS ER120S-G and AWS ER100S-G, according to manufacturer.
Table 2. Chemical composition of AWS ER120S-G and AWS ER100S-G, according to manufacturer.
Chemical Composition of AWS ER120S-G in Weight %
CSiMnNiCrMo
0.0810.801.752.220.410.53
Chemical Composition of AWS ER100S-G in Weight %
CSiMnNiCrMo
0.120.711.380.530.580.20
Table 3. Welding modes and parameters at different welding gaps.
Table 3. Welding modes and parameters at different welding gaps.
Welding Mode (W)Welding Gap, mmPass №Current I, AVoltage U, VWelding Rate, mm/minScheme of Welding Sequences
W10124031280Materials 17 04534 i001
227031150
W24124031250Materials 17 04534 i002
224031180
327032140
W36124031250Materials 17 04534 i003
224031180
327032.5120
W48124031250Materials 17 04534 i004
224031180
324031180
427032.5100
Table 4. Some electrochemical characteristics of the tested specimens.
Table 4. Some electrochemical characteristics of the tested specimens.
Welding ModeEss, mVEcorr, mVicorr, mA/cm2CR, mm/yrMicrostructure
S960QLS700MCS960QLS700MCS960QLS700MCS960QLS700MCS960QLS700MC
Base metal−435−375−476−3573.47 × 10−11.40 × 10−24.040.16M + BF + B
W1−415−425−440−4146.80 × 10−21.30 × 10−10.791.50M + Aret. + Fal.M + Aret. + Fid.
W2−320−425−458−4214.46 × 10−21.40 × 10−10.521.58
W3−346−424−494−4175.56 × 10−21.60 × 10−10.651.85
W4−416−415−481−4284.43 × 10−23.30 × 10−10.523.81
Ess—steady state potential; Ecorr—corrosion potential; icorr—corrosion current density; CR—corrosion penetration rate; M—martensite; Aret.—retained austenite; B—bainite; Fal.—allotriomorphic ferrite; Fid.—idiomorphic ferrite.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Ilieva, M.; Gospodinov, D.; Ferdinandov, N.; Radev, R. Corrosion Behaviour of Weld Metal of Ultra-High-Strength Steel Weldments in a Sodium Chloride Aqueous Solution. Materials 2024, 17, 4534. https://doi.org/10.3390/ma17184534

AMA Style

Ilieva M, Gospodinov D, Ferdinandov N, Radev R. Corrosion Behaviour of Weld Metal of Ultra-High-Strength Steel Weldments in a Sodium Chloride Aqueous Solution. Materials. 2024; 17(18):4534. https://doi.org/10.3390/ma17184534

Chicago/Turabian Style

Ilieva, Mariana, Danail Gospodinov, Nikolay Ferdinandov, and Rossen Radev. 2024. "Corrosion Behaviour of Weld Metal of Ultra-High-Strength Steel Weldments in a Sodium Chloride Aqueous Solution" Materials 17, no. 18: 4534. https://doi.org/10.3390/ma17184534

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop