Next Article in Journal
Neo-Geometric Copper Nanocrystals by Competitive, Dual Surfactant-Mediated Facet Adsorption Controlling Skin Permeation
Next Article in Special Issue
An Analytical Calculation of Frictional and Bending Moments at the Head-Neck Interface of Hip Joint Implants during Different Physiological Activities
Previous Article in Journal
Acoustic Behavior of Hollow Blocks and Bricks Made of Concrete Doped with Waste-Tire Rubber
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Tribocorrosion Failure Mechanism of TiN/SiOx Duplex Coating Deposited on AISI304 Stainless Steel

1
Southwest Technology and Engineering Research Institute, Chongqing 400039, China
2
School of Mechanical Engineering and Automation, University of Science and Technology Liaoning, Anshan 114051, China
3
Chongqing Institute of Green and Intelligent Technology, Chinese Academy of Sciences, Chongqing 400714, China
4
Guangdong Provincial Key Laboratory of Micro/Nano Optomechatronics Engineering, Shenzhen University, Shenzhen 518060, China
*
Authors to whom correspondence should be addressed.
Materials 2016, 9(12), 963; https://doi.org/10.3390/ma9120963
Submission received: 11 October 2016 / Revised: 13 November 2016 / Accepted: 21 November 2016 / Published: 26 November 2016

Abstract

:
TiN/SiOx duplex coatings were synthesized on AISI304 stainless steel by plasma immersion ion implantation and deposition (PIIID) followed by radio frequency magnetron sputtering (RFMS). The microstructure and tribocorrosion failure behaviors of the duplex coatings were investigated by X-ray diffraction, X-ray photoelectron spectroscopy, scanning electron microscopy, atomic force microscopy, reciprocating-sliding tribometer, and electrochemical tests. The as-deposited duplex coating had a two-layered columnar growth structure consisting of face-centered cubic TiN and amorphous SiOx. Sliding tests showed that the TiN interlayer had good adhesion with the substrate, but the SiOx layer suffered from severe delamination failure. Friction force induced a number of micro-cracks in the coating, which provided channels for the diffusion of NaCl solution. The tribocorrosion test showed that the duplex coating exhibited a lower wear-performance in NaCl solution than in ambient atmosphere. Multi-scale chloride ion corrosion occurred simultaneously and substantially degraded the bonding strength of the columnar crystals or neighboring layers. Force-corrosion synergy damage eventually led to multi-degradation failure of the duplex coating. The presented results provide a comprehensive understanding of the tribocorrosion failure mechanism in coatings with duplex architecture.

1. Introduction

In view of its low cost, ease of manufacturing, excellent mechanical properties, and corrosion resistance, stainless steel is the most popularly used material in artificial implants [1,2,3]. However, the synergistic effect of severe chloride ion corrosion and wear-corrosion greatly affects the reliability and service life of stainless steel in chloride ion-rich corrosive media [4,5,6,7]. Therefore, it is necessary to develop protective coatings that have both anti-wear and anti-corrosion properties.
Nitrides, carbides, and oxides are promising materials for protective coatings against wear and corrosion. For instance, stainless steels coated with CrCN showed enhanced corrosion resistance and wear resistance [8]. TiN coatings greatly improved the wear resistance and corrosion resistance of stainless steel in simulated body fluid (SBF) solution [9,10]. Ti-O-N, SiOx and TiBxCy/a-C coatings are also candidates for potential applications in biomedical sectors due to their good corrosion resistance and wear resistance [11,12,13]. However, these single coatings suffered from severe delamination failure in corrosive media due to micro-crack propagation [13,14]. Recent results reported that coatings with duplex architecture could effectively prevent micro-crack propagation and such coatings showed better tribocorrosion performances compared to single component coatings [14,15,16,17], indicating a feasible strategy to design protective coatings for tribocorrosion applications.
Tribocorrosion is defined as degradation due to the combined effect of mechanical wear and electrochemical corrosion [18,19,20,21]. This synergistic damage is often more intense than wear and/or anodic dissolution alone [22]. Li et al. [23,24] reported that TiSiN and TiCN showed a higher wear rate in seawater than in air. Wang [14] reported that micro-cracks played an important role in determining the rate of delamination of a coating. However, the mechanism of damage due to the synergistic wear-corrosion effect is still not clearly known. Si element is an essential trace element for the normal growth and development of bone. Si-containing coatings show good prospects for application in biomedical implants (e.g., hip and knee). However, there are only few studies on the tribocorrosion failure mechanism of Si-containing coatings in a chloride ion-rich corrosive environment. Here a TiN/SiOx duplex coating was designed to enhance the wear resistance and corrosion resistance of stainless steel. The purpose of the TiN interlayer is to retard chloride ion corrosion and provide load support for the top layer of SiOx. The tribocorrosion failure behavior of the as-deposited coating was investigated in NaCl solution. The synergistic damage mechanism of wear-corrosion in the duplex coating is also discussed.

2. Materials and Methods

The TiN/SiOx duplex coating was synthesized using a multi-purpose plasma immersion ion implantation and deposition facility, where continuous plasma immersion ion implantation and deposition (PIIID) and radio frequency magnetron sputtering (RFMS) processes can be carried out without breaking vacuum [25,26,27]. The AISI304 stainless steel was used as the substrate. All the samples were mechanically polished using diamond paste (average particle size of 20 μm) followed by ultrasonic cleaning in pure ethanol. High purity Ti and Si were used as the targets. High purity Ar (99.999%), N2 (99.999%), and O2 (99.999%) were used to provide the working atmosphere. During the experiment, the vacuum chamber was evacuated to a base pressure of 0.005 Pa. Prior to the deposition of the coating, the polished samples were cleaned by Ar+ sputtering at a bias voltage of 6 kV for 30 min to remove residual pollution. The TiN layer was deposited in a N2 atmosphere. The experimental parameters were as follows: pressure 0.3 Pa, bias voltage 20 kV, frequency 75 Hz, bias voltage duration 60 µs, and deposition time 2 h. Subsequently, the SiOx layer was deposited in Ar and O2 atmosphere by RFMS with the following experimental parameters: pressure 2 Pa, bias voltage 6 kV, frequency 100 Hz, bias voltage duration 60 µs, RF power 400 W, and deposition time 2 h.
The crystalline structure of the coating was determined by X-ray diffraction (XRD, X’pert Powder, PANalytical, Almelo, The Netherlands) using a Cu Kα radiation source. The diffraction angle ranged from 20° to 90° and a scanning rate of 0.1°/s was used. The measurement was conducted with an incidence angle of 0.8°, a voltage of 40 kV, and a current of 40 mA. The scan step and integration time were 1400 and 0.5 s, respectively. The chemical bonding states of the component layers were detected by X-ray photoelectron spectroscopy (XPS, Thermo, K-Alpha, Waltham, MA, USA) using Al Kα radiation as the excitation source. Argon ion etching (accelerating voltage 1000 eV) was performed to remove contaminants. A field emission scanning electron microscopy (SEM, JSM-6701F, JEOL, Tokyo, Japan) was used to observe the cross-sectional morphology of the coating. The surface roughness of the coating was determined using an atomic force microscope (AFM, Dimension 3100, Veeco Instruments Inc., Plainview, NY, USA) in contact mode. The surface roughness (Ra) was obtained for a scanned area of 4 μm2. The mechanical properties of the component layers were evaluated by a nano-indentation system (Nano Indenter® G200, Palo Alto, CA, USA). The hardness (H) and elastic modulus (E) were calculated using the Oliver-Pharr method [28]. The corrosion behavior of the coatings in 3.5 wt % NaCl solution was investigated electrochemically (PGSTAT302N, Herisau, Switzerland). High purity platinum was used as the counter electrode, the sample as the working electrode (1 cm2 exposed areas) and a saturated calomel electrode (SCE) as the reference electrode. The electrochemical tests were conducted in potentiostatic mode. The potential range and scanning rate were ±250 mV and 1 mV/s, respectively. Each test was repeated three times to ensure reproducibility.
A reciprocating sliding tribometer (MFT-R4000, Lanzhou Institute of Chemical Physics, Chinese Academy of Sciences, Lanzhou, China) was employed to evaluate the tribocorrosion failure behaviors of the coating in a 3.5 wt % NaCl solution. As shown in Figure 1, high purity graphite was used as the counter electrode, the sample as the working electrode and a saturated calomel electrode (SCE) as the reference electrode. During the tribocorrosion test, the open circuit potential (OCP) was recorded for 5 min prior to sliding after which the sliding test was continued for 15 min. A load of 5 N was applied on the sample using an Al2O3 ball (Φ 6 mm). The initial Hertzian contact pressure was about 0.987 GPa. The amplitude and frequency were 5 mm and 0.1 Hz, respectively. The OCP recording was continued for 5 min after the sliding had ended. The sliding test under atmosphere was also conducted under the same conditions for 15 min in order to investigate the wear-corrosion synergistic damage mechanisms. Each test was repeated three times under the same conditions in order to check the reproducibility. The “mean by cycle” values of the friction coefficients were used to evaluate the wear performance of the duplex coating. The wear track surface morphologies and the chemical composition of the coatings after the sliding tests were examined by SEM.

3. Results and Discussion

Figure 2 shows the XRD pattern of the TiN/SiOx duplex coating. It can be seen that the Bragg refection peaks located at 36.71°, 42.63°, and 61.97° can be assigned to reflections from (111), (200) and (220) planes respectively, of face-centered cubic TiN [29]. No obvious diffraction peaks for silicon oxide phases were identified in this coating, indicating that the top SiOx layer is amorphous or poorly crystallized.
Figure 3 presents the XPS spectrum of the TiN and SiOx component layers. As shown in Figure 3a,b, the binding energies of Ti2p3/2 and N1s peaks are at 455.2 eV and 397.3 eV, respectively, which are attributed to the presence of the TiN [30]. These results are in good agreement with the XRD characterization (see Figure 2). The binding energies of Si2p (Figure 3c) and O1s (Figure 3d) are centered at 103.1 eV and 532.5 eV, respectively, indicating that silicon in the coating is bound to oxygen [31].
Figure 4 shows the cross-sectional SEM image of the TiN/SiOx duplex coating. A clear two-layered structure is observed and all the component layers exhibit typical columnar growth. However, the TiN interlayer consists of more densely packed and refined crystals compared to the SiOx layer. The thickness of the TiN and SiOx layers are 325 nm and 298 nm, respectively.
Figure 5 shows the AFM surface morphologies of the component layers. As shown in Figure 5a, the surface roughness (Ra) of the TiN interlayer is 1.49 nm, indicating that this layer is smoother than that of the SiOx layer (Figure 5b, Ra = 2.77 nm).
Figure 6 shows the anode polarization curves and corrosion images of the substrate and TiN/SiOx duplex coating. As shown in Figure 6a, the corrosion potential and corrosion current density of the substrate are −317 ± 43 mV and 1.64 ± 0.31 × 10−7 A/cm2, respectively. The corresponding image reveals that a large number of corrosion pores are found distributed on the substrate surface. The TiN/SiOx duplex coating exhibits a better corrosion resistance with a higher corrosion potential of −272 ± 31 mV and a lower corrosion current density of 1.72 ± 0.49 × 10−8 A/cm2 (Figure 6b). This coating exhibits a smooth morphology and few corrosion defects are observed, indicating the excellent corrosion protection capability of the coating for the substrate.
Figure 7 shows the nano-indentation curves of the component layers. The hardness, elastic modulus and H/E value of the TiN layer are 19.80 ± 0.35 GPa, 186.7 ± 9.54 GPa and 0.106, respectively. The SiOx layer shows a hardness of 5.2 ± 0.72 GPa, an elastic modulus of 110.9 ± 12.41 GPa and an H/E value of 0.047. Nano-indentation results confirm that the TiN interlayer exhibits better mechanical properties as compared to the SiOx layer.
Figure 8a presents the variation of the friction coefficient of the TiN/SiOx duplex coating during sliding tests. This coating exhibits a relatively stable wear performance in air with a constant friction coefficient of 0.18 during the whole sliding cycle. However, the coating shows an unstable wear performance in NaCl solution. The friction coefficient increases gradually and reaches the maximum value of 0.55 at the end of 80 sliding cycles. Figure 8b is a typical tribocorrosion curve showing the variation in OCP of the TiN/SiOx duplex coating in NaCl solution. It can be seen that this coating exhibits a relatively stable OCP value of −0.05 V during the soaking, but the OCP value decreases by 0.55 V during tribocorrosion and increases gradually to −0.38 V during passivation. Moreover, the decline in OCP value is proportional to the increase in frictional force, indicating the intense wear-corrosion synergistic effect.
Figure 9 shows the typical cross-sectional profiles of the wear track after the sliding test. When tested in air, the TiN/SiOx duplex coating exhibits a chunk peeling profile under atmosphere with a wear track width of 198 μm and a wear track depth of 294 nm (Figure 9a). The wear track profile shown in Figure 9b reveals that the TiN/SiOx duplex coating suffers from severe wear in NaCl solution and the wear track is wider (396 μm). The maximum wear track depth is up to 795 nm (marked by arrows). By referring to the corresponding component layer (see Figure 4), it can be inferred that the stable friction coefficient in air atmosphere involves only the SiOx layer. However, the unstable friction coefficient in NaCl solution indicates that both the substrate and the TiN interlayer are involved during tribocorrosion.
Figure 10 shows the SEM image and energy dispersive spectroscopy (EDS) analysis of the wear track after sliding tests in air. The wear track shows a number of coating spallings and peelings (Figure 10a). The strong Si peak identified in zone 1 indicates that the peeling occurs in the SiOx layer (Figure 10b). The SEM image (insert in Figure 10b) reveals that the SiOx layer undergoes failure by particle fragmentation. EDS analysis of zone 2 reveals a strong Ti peak and a weak Si peak, confirming that the wear occurs in the TiN interlayer for this zone (Figure 10c). The high-resolution SEM image in Figure 10c shows that the wear track is characterized by a large number of parallel cracks.
Figure 11 shows the SEM image and EDS analysis of the wear track after the tribocorrosion test. It can be seen that severe coating delamination and tribocorrosion damages appear in the wear track (Figure 11a). The strong Ti peaks indentified in zone 1 confirm that the SiOx layer tends to delaminate from the TiN interlayer (Figure 11b). The EDS analysis of zone 2 reveals the presence of Fe, Cr, Ni, and Si, whereas Ti is absent in this zone (Figure 11c). These results imply that the delamination failure occurs at the interface of the TiN interlayer with the substrate. Micro-pores observed in the failure zone confirm the occurrence of severe pitting corrosion (SEM image inset in Figure 11c). The strong Si peak identified in zone 3 proves that the SiOx layer does not show wear failure, but undergoes intense tribocorrosion damage with severe warp and fracture (SEM image inset in Figure 11d). These failure characteristics are clearly different from those shown in Figure 10b.
Figure 12 shows the high-resolution SEM image and EDS analysis of the plough after tribocorrosion test. A number of parallel and penetrating cracks are observed on the surface of the plough (Figure 12a). The presence of Fe, Cr, Ni, and Si in zone 1 indicates that the TiN/SiOx duplex coating has worn out (Figure 12b). The strong Ti peak identified in zone 2 conforms that the tribocorrosion occurs in the TiN interlayer (Figure 12c). The presence of penetrating cracks in this coating, in contrast to the wear track in air (Figure 10c), confirms that the TiN interlayer suffers more severe damage in NaCl solution.
The sliding test shows that the TiN interlayer exhibits excellent adhesion with the substrate, whereas the SiOx layer undergoes severe delamination failure. These failure characteristics can be attributed to the differences in the mechanical properties of the component layers. As shown in Figure 7, the H/E value of the TiN interlayer is 0.106, which is higher than that of the SiOx layer (0.047). It is generally believed that the ability of a coating to resist mechanical degradation and fracture is improved by high hardness, low elastic modulus and a high H/E ratio [32,33]. Therefore, the soft SiOx layer suffers from severe fracture failure due to its poor fracture resistance.
The tribocorrosion test confirms that the TiN/SiOx duplex coating shows a lower wear resistance in NaCl solution than in air. Plenty of penetrating cracks and layered delamination appear on the wear track (Figure 11). These multi-degradation failures mainly originate from force-corrosion synergy damage. As shown in Figure 4, this coating has a typical columnar growth structure, which benefits the initiation and propagation of micro-cracks along the columnar boundaries. Frictional force induces a large number of parallel cracks in the coating (see SEM images in Figure 10b,c). These micro-cracks provide channels and thereby accelerate the diffusion of NaCl solution. It has been reported that chloride ion plays a major role in inducing the pitting corrosion of materials [34,35]. The visible micro-pores and the presence of elemental Cl in the wear track confirm the simultaneous chloride ion corrosion during the tribocorrosion (see Figure 11c). This multi-scale chloride ion corrosion greatly degrades the bonding strength between the columnar crystals and the adjacent layers (e.g., substrate/TiN and TiN/SiOx). Consequently, the intense force-corrosion synergy interaction leads to a severe multi-degradation failure of the TiN/SiOx duplex coating.

4. Conclusions

This study investigated the tribocorrosion failure behavior of TiN/SiOx duplex coatings in NaCl solution; the main conclusions are as follows:
(1).
The TiN/SiOx duplex coating has a two-layered columnar growth structure which is made up of a face-centered cubic TiN interlayer and a layer of amorphous SiOx, and provides excellent corrosion protection to the stainless steel substrate.
(2).
The TiN interlayer exhibits good adhesion with the substrate, but the SiOx layer suffers from severe delamination failure during the sliding test in air.
(3).
Frictional force induces a large number of micro-cracks in the TiN/SiOx duplex coating. These micro-cracks provide diffusion channels for the NaCl solution and eventually cause simultaneous chloride ion corrosion during the tribocorrosion.
(4).
The multi-scale Cl ion corrosion greatly weakens the bonding strength of the columnar crystals or the adjacent layers. The force-corrosion synergy interaction damage induces multi-degradation failures in the TiN/SiOx duplex coating.
Our results confirm that synergistic wear-corrosion damage greatly accelerates the failure of the duplex coating. It is therefore important to choose coating materials that have a high H/E ratio as well as a dense structure to design future biomedical duplex coatings.

Acknowledgments

This work is supported by National Natural Science Foundation of China (No. 51401201), Liaoning BaiQianWan Talents Program (201571), Natural Science Foundation of Liaoning Province (201602392), Program for Liaoning Excellent Talents in University (LJQ2015052), Excellent Talents Program of University of Science and Technology Liaoning (2014RC04) and Chongqing Research of Application Foundation and Advanced Technology (cstc2014jcyjA50009).

Author Contributions

Qiang Chen and Zhiwen Xie designed the experiments and wrote the paper. Tian Chen performed the experiments. Feng Gong analyzed the data.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Jin, Z.H.; Ge, H.H.; Lin, W.W.; Zong, Y.W.; Liu, S.J.; Shi, J.M. Corrosion behaviour of 316L stainless steel and anti-corrosion materials in a high acidified chloride solution. Appl. Surf. Sci. 2014, 322, 47–56. [Google Scholar] [CrossRef]
  2. Naghizadeh, M.; Nakhaie, D.; Zakeri, M.; Moayed, M.H. The effect of dichromate ion on the pitting corrosion of AISI 316 stainless steel Part II: Pit initiation and transition to stability. Corros. Sci. 2015, 94, 420–427. [Google Scholar] [CrossRef]
  3. Pacquentin, W.; Carona, N.; Oltra, R. Effect of microstructure and chemical composition on localized corrosion resistance of a AISI 304L stainless steel after nanopulsed-laser surface melting. Appl. Surf. Sci. 2015, 356, 561–573. [Google Scholar] [CrossRef]
  4. Von der Ohe, C.B.; Johnsen, R.; Espallargas, N. Multi-degradation behavior of austenitic and super duplex stainless steel—The effect of 4-point static and cyclic bending applied to a simulated seawater tribocorrosion system. Wear 2012, 288, 39–53. [Google Scholar] [CrossRef]
  5. Sun, Y.; Rana, V. Tribocorrosion behaviour of AISI 304 stainless steel in 0.5 M NaCl solution. Mater. Chem. Phys. 2011, 129, 138–147. [Google Scholar] [CrossRef]
  6. Silva, R.C.C.; Nogueira, R.P.; Bastos, I.N. Tribocorrosion of UNS S32750 in chloride medium: Effect of the load level. Electrochim. Acta 2011, 56, 8839–8845. [Google Scholar] [CrossRef]
  7. López, A.; Bayón, R.; Pagano, F.; Igartua, A.; Arredondo, A.; Arana, J.L.; González, J.J. Tribocorrosion behaviour of mooring high strength low alloy steels in synthetic seawater. Wear 2015, 338–339, 1–10. [Google Scholar] [CrossRef]
  8. Ye, Y.W.; Wang, Y.X.; Wang, C.T.; Li, J.L.; Yao, Y.R. An analysis on tribological performance of CrCN coatings with different carbon contents in seawater. Tribol. Int. 2015, 91, 131–139. [Google Scholar] [CrossRef]
  9. Wang, Y.; Northwood, D.O. Effect of substrate material on the corrosion of TiN-coated stainless steels in simulated anode and cathode environments of proton exchange membrane fuel cells. J. Power Sources 2009, 191, 483–488. [Google Scholar] [CrossRef]
  10. Wang, L.; Su, J.F.; Nie, X. Corrosion and tribological properties and impact fatigue behaviors of TiN- and DLC-coated stainless steels in a simulated body fluid environment. Surf. Coat. Technol. 2010, 205, 1599–1605. [Google Scholar] [CrossRef]
  11. Sun, T.; Wang, L.P.; Wang, M. Characteristics and mechanical properties of a (Ti, O, N)/Ti composite coating fabricated on NiTi shape memory alloy via PIIID. Mater. Lett. 2010, 64, 1769–1771. [Google Scholar] [CrossRef]
  12. Kuo, Y.L.; Chang, K.H. Atmospheric pressure plasma enhanced chemical vapor deposition of SiOx films for improved corrosion resistant properties of AZ31 magnesium alloys. Surf. Coat. Technol. 2015, 283, 194–200. [Google Scholar] [CrossRef]
  13. Gracia-Escosa, E.; García, I.; Sánchez-López, J.C.; Abad, M.D.; Mariscal, A.; Arenas, M.A.; de Damborenea, J.; Conde, A. Tribocorrosion behavior of TiBxCy/a-C nanocomposite coating in strong oxidant disinfectant solutions. Surf. Coat. Technol. 2015, 263, 78–85. [Google Scholar] [CrossRef]
  14. Shan, L.; Wang, Y.X.; Li, J.L.; Jiang, X.; Chen, J.M. Improving tribological performance of CrN coatings in seawater by structure design. Tribol. Int. 2015, 82, 78–88. [Google Scholar] [CrossRef]
  15. Rossi, S.; Fedrizzi, L.; Leoni, M.; Scardi, P.; Massiani, Y. (Ti, Cr)N and Ti/TiN PVD coatings on 304 stainless steel substrates: Wear-corrosion behavior. Thin Solid Films 1999, 350, 161–167. [Google Scholar] [CrossRef]
  16. Naghibi, S.A.; Raeissi, K.; Fathi, M.H. Corrosion and tribocorrosion behavior of Ti/TiN PVD coating on 316L stainless steel substrate in Ringer’s solution. Mater. Chem. Phys. 2014, 148, 614–623. [Google Scholar] [CrossRef]
  17. Sun, T.; Xue, N.; Liu, C.; Wang, C.; He, J. Bioactive (Si, O, N)/(Ti, O, N)/Ti composite coating on NiTi shapememory alloy for enhanced wear and corrosion performance. Appl. Surf. Sci. 2015, 356, 599–609. [Google Scholar] [CrossRef]
  18. Lemaire, E.; le Calvar, M. Evidence of tribocorrosion wear in pressurized water reactors. Wear 2001, 249, 338–344. [Google Scholar] [CrossRef]
  19. Mischler, S. Triboelectrochemical techniques and interpretation methods in tribocorrosion: A comparative evaluation. Tribol. Int. 2008, 41, 573–583. [Google Scholar] [CrossRef]
  20. Sun, Y.; Bailey, R. Improvement in tribocorrosion behavior of 304 stainless steel by surface mechanical attrition treatment. Surf. Coat. Technol. 2014, 253, 284–291. [Google Scholar] [CrossRef]
  21. Kok, Y.N.; Akid, R.; Hovsepian, P.E. Tribocorrosion testing of stainless steel (SS) and PVD coated SS using a modified scanning reference electrode technique. Wear 2005, 259, 1472–1481. [Google Scholar] [CrossRef]
  22. Landolt, D.; Mischler, S.; Stemp, M. Electrochemical methods in tribocorrosion: A critical appraisal. Electrochim. Acta 2001, 46, 3913–3929. [Google Scholar] [CrossRef]
  23. Yao, Y.R.; Li, J.L.; Wang, Y.X.; Ye, Y.W.; Zhu, L.H. Influence of the negative bias in ion plating on the microstructural and tribological performances of Ti-Si-N coatings in seawater. Surf. Coat. Technol. 2015, 280, 154–162. [Google Scholar] [CrossRef]
  24. Shan, L.; Wang, Y.X.; Li, J.L.; Li, H.; Wu, X.D.; Chen, J.M. Tribological behaviours of PVD TiN and TiCN coatings in artificial seawater. Surf. Coat. Technol. 2013, 226, 40–50. [Google Scholar] [CrossRef]
  25. Wang, L.P.; Huang, L.; Xie, Z.W.; Wang, X.F.; Tang, B.Y. Fourth-generation plasma immersion ion implantation and deposition facility for hybrid surface modification layer fabrication. Rev. Sci. Instrum. 2008, 79, 023306. [Google Scholar] [CrossRef] [PubMed]
  26. Xie, Z.W.; Chen, Q.; Chen, T.; Gao, X.; Yu, X.G.; Song, H.; Feng, Y.J. Microstructure and properties of nitrogen ion implantation/AlN/CrAlN/MoS2-phenolic resin duplex coatings on magnesium alloys. Mater. Chem. Phys. 2015, 160, 212–220. [Google Scholar] [CrossRef]
  27. Chen, T.; Xie, Z.W.; Gong, F.; Luo, Z.Z.; Yang, Z. Correlation between microstructure evolution and high temperature properties of TiAlSiN hard coatings with different Si and Al content. Appl. Surf. Sci. 2014, 314, 735–745. [Google Scholar] [CrossRef]
  28. Oliver, W.C.; Pharr, G.M. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. J. Mater. Res. 1992, 7, 1564–1583. [Google Scholar] [CrossRef]
  29. Chen, L.; Du, Y.; Mayrhofer, P.H.; Wang, S.Q.; Li, J. The influence of age-hardening on turning and milling performance of Ti-Al-N coated inserts. Surf. Coat. Technol. 2008, 202, 5158–5161. [Google Scholar] [CrossRef]
  30. Yu, D.H.; Wang, C.Y.; Cheng, X.L.; Zhang, F.L. Microstructure and properties of TiAlSiN coatings prepared by hybrid PVD technology. Thin Solid Films 2009, 517, 4950–4955. [Google Scholar] [CrossRef]
  31. Liu, Z.; Ma, X.X.; Yang, C.L.; Xu, F.J. Characterization of composite SiOx/polymer films deposited on pet substrates by RF reactive magnetron sputtering. Vacuum 2013, 89, 109–112. [Google Scholar] [CrossRef]
  32. Leyland, A.; Matthews, A. On the significance of the H/E ratio in wear control: Ananocomposite coating approach to optimised tribological behavior. Wear 2000, 246, 1–11. [Google Scholar] [CrossRef]
  33. Lin, J.L.; Moore, J.J.; Mishra, B.; Pinkas, M.; Sproul, W.D. The structure and mechanical and tribological properties of TiBCN nanocomposite coatings. Acta Mater. 2010, 58, 1554–1564. [Google Scholar] [CrossRef]
  34. Wang, Y.F.; Cheng, G.X.; Wu, W.; Qiao, Q.; Li, Y.; Li, X.F. Effect of pH and chloride on the micro-mechanism of pitting corrosion for high strength pipeline steel in aerated NaCl solutions. Appl. Surf. Sci. 2015, 349, 746–756. [Google Scholar] [CrossRef]
  35. Bhandari, J.; Khan, F.; Abbassi, R.; Garaniy, V.; Ojeda, R. Modelling of pitting corrosion in marine and off shore steel structures-A technical review. J. Loss Prevent. Proc. 2015, 37, 39–62. [Google Scholar] [CrossRef]
Figure 1. Scheme of the tribocorrosion apparatus.
Figure 1. Scheme of the tribocorrosion apparatus.
Materials 09 00963 g001
Figure 2. XRD pattern of the TiN/SiOx duplex coating.
Figure 2. XRD pattern of the TiN/SiOx duplex coating.
Materials 09 00963 g002
Figure 3. XPS spectrum of the TiN and SiOx component layers: (a) Ti2p; (b) N1s; (c) Si2p; (d) O1s.
Figure 3. XPS spectrum of the TiN and SiOx component layers: (a) Ti2p; (b) N1s; (c) Si2p; (d) O1s.
Materials 09 00963 g003
Figure 4. Cross-sectional SEM image of the TiN/SiOx duplex coating.
Figure 4. Cross-sectional SEM image of the TiN/SiOx duplex coating.
Materials 09 00963 g004
Figure 5. AFM surface morphologies of the component layers: (a) TiN interlayer; (b) SiOx layer.
Figure 5. AFM surface morphologies of the component layers: (a) TiN interlayer; (b) SiOx layer.
Materials 09 00963 g005
Figure 6. Anode polarization curves and corrosion morphologies of (a) substrate and (b) TiN/SiOx duplex coating.
Figure 6. Anode polarization curves and corrosion morphologies of (a) substrate and (b) TiN/SiOx duplex coating.
Materials 09 00963 g006
Figure 7. Nanoindentation curves of the component layers.
Figure 7. Nanoindentation curves of the component layers.
Materials 09 00963 g007
Figure 8. (a) Friction coefficient of the TiN/SiOx duplex coating; (b) a typical tribocorrosion curve with the OCP values of the TiN/SiOx duplex coating in NaCl solution.
Figure 8. (a) Friction coefficient of the TiN/SiOx duplex coating; (b) a typical tribocorrosion curve with the OCP values of the TiN/SiOx duplex coating in NaCl solution.
Materials 09 00963 g008
Figure 9. Cross-sectional profiles of the wear track after sliding test: (a) in air; (b) in NaCl solution.
Figure 9. Cross-sectional profiles of the wear track after sliding test: (a) in air; (b) in NaCl solution.
Materials 09 00963 g009
Figure 10. (a) SEM wear track image of the TiN/SiOx duplex coating in air; (b) EDS analysis of zone 1; (c) EDS analysis of zone 2.
Figure 10. (a) SEM wear track image of the TiN/SiOx duplex coating in air; (b) EDS analysis of zone 1; (c) EDS analysis of zone 2.
Materials 09 00963 g010
Figure 11. (a) SEM images of wear track in TiN/SiOx duplex coating in NaCl solution; (b) EDS analysis of zone 1; (c) EDS analysis of zone 2; (d) EDS analysis of zone 3.
Figure 11. (a) SEM images of wear track in TiN/SiOx duplex coating in NaCl solution; (b) EDS analysis of zone 1; (c) EDS analysis of zone 2; (d) EDS analysis of zone 3.
Materials 09 00963 g011
Figure 12. (a) High resolution SEM image of the tribocorrosion plough; (b) EDS analysis of zone 1; (c) EDS analysis of zone 2.
Figure 12. (a) High resolution SEM image of the tribocorrosion plough; (b) EDS analysis of zone 1; (c) EDS analysis of zone 2.
Materials 09 00963 g012

Share and Cite

MDPI and ACS Style

Chen, Q.; Xie, Z.; Chen, T.; Gong, F. Tribocorrosion Failure Mechanism of TiN/SiOx Duplex Coating Deposited on AISI304 Stainless Steel. Materials 2016, 9, 963. https://doi.org/10.3390/ma9120963

AMA Style

Chen Q, Xie Z, Chen T, Gong F. Tribocorrosion Failure Mechanism of TiN/SiOx Duplex Coating Deposited on AISI304 Stainless Steel. Materials. 2016; 9(12):963. https://doi.org/10.3390/ma9120963

Chicago/Turabian Style

Chen, Qiang, Zhiwen Xie, Tian Chen, and Feng Gong. 2016. "Tribocorrosion Failure Mechanism of TiN/SiOx Duplex Coating Deposited on AISI304 Stainless Steel" Materials 9, no. 12: 963. https://doi.org/10.3390/ma9120963

APA Style

Chen, Q., Xie, Z., Chen, T., & Gong, F. (2016). Tribocorrosion Failure Mechanism of TiN/SiOx Duplex Coating Deposited on AISI304 Stainless Steel. Materials, 9(12), 963. https://doi.org/10.3390/ma9120963

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop