Next Article in Journal / Special Issue
Catalytic Abatement of Nitrous Oxide Coupled with Ethane Oxydehydrogenation over Mesoporous Cr/Al2O3 Catalyst
Previous Article in Journal
Photocatalytic Graphene-TiO2 Thin Films Fabricated by Low-Temperature Ultrasonic Vibration-Assisted Spin and Spray Coating in a Sol-Gel Process
Previous Article in Special Issue
A Study of Low-Temperature CO Oxidation over Mesoporous CuO-TiO2 Nanotube Catalysts
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Cobalt-iron Oxide, Alloy and Nitride: Synthesis, Characterization and Application in Catalytic Peroxymonosulfate Activation for Orange II Degradation

1
Mössbauer Effect Data Center, Dalian Institute of Chemical Physics, Chinese Academy of Sciences, Dalian 116023, China
2
University of Chinese Academy of Sciences, Beijing 100049, China
3
Nuclear Analysis and Radiography Department, Institute for Energy Security and Environmental Safety, Centre for Energy Research, Hungarian Academy of Sciences, Konkoly Thege Miklós út 29-33, 1121 Budapest, Hungary
*
Author to whom correspondence should be addressed.
Catalysts 2017, 7(5), 138; https://doi.org/10.3390/catal7050138
Submission received: 27 February 2017 / Revised: 4 April 2017 / Accepted: 24 April 2017 / Published: 4 May 2017
(This article belongs to the Special Issue Heterogeneous Catalysis for Environmental Remediation)

Abstract

:
In meeting the need for environmental remediation in wastewater treatment and the development of popular sulfate-radical-based advanced oxidation processes (SR-AOPs), a series of Co/Fe-based catalysts with confirmed phase structure were prepared through extended soft chemical solution processes followed by atmosphere-dependent calcination. Powder X-ray diffraction (XRD), scanning electron microscopy (SEM), transmission electron microscopy (TEM), X-ray photoelectron spectroscopy (XPS) and 57Fe Mössbauer spectroscopy were employed to characterize the composition, morphology, crystal structure and chemical state of the prepared catalysts. It was shown that calcination in air, nitrogen and ammonia atmospheres generated Co-Fe catalysts with cobalt ferrite (CoFe2O4), Co-Fe alloy and Co-Fe nitride as dominant phases, respectively. The prepared Co/Fe-based catalysts were demonstrated to be highly efficient in activating peroxymonosulfate (PMS) for organic Orange II degradation. The activation efficiency of the different catalysts was found to increase in the order CoFe2O4 < Co-Fe nitride < Co-Fe alloy. Sulfate radical was found to be the primary active intermediate species contributing to the dye degradation for all the participating catalysts. Furthermore, a possible reaction mechanism was proposed for each of the studied catalysts. This study achieves progress in efficient cobalt-iron catalysts using in the field of SR-AOPs, with potential applications in environment remediation.

Graphical Abstract

1. Introduction

Industries such as textiles, printing, plastics, pharmaceuticals, rubber, etc., may bring great threats to the water environment, owing to the production of lots of organic pollutants, most of which are carcinogenic, teratogenic, mutagenic and resistant to biodegradation [1]. Thus, advanced oxidation processes (AOPs) have been developed to solve the wastewater issues, which have been attractive techniques for the realization of powerful degradation ability. As classic active species, hydroxyl radical (·OH) generated during the oxidation processes has been widely investigated because of its remarkable reactivity towards almost all the organic compounds [2]. However, it may suffer from limitations such as pH value dependence, slow reaction rate, sludge generation and difficulties regarding the safety of storage and transportation of the oxidant—hydrogen peroxide (H2O2). Recently, on account of their superior oxidation ability, good safety, wide range of pH conditions, sulfate-radical-based advanced oxidation processes (SR-AOPs) have emerged as a promising technique and a favorable alternative to H2O2 based organics degradation processes [3].
With respect to other transition-metal-based catalysts, cobalt ions and their composites were reported to be more efficient as peroxymonosulfate (PMS) activators in most organic pollutant degradations [4]. Since the first report about Co2+ catalytic decomposition of PMS, homogeneous processes on different Co2+ counteranions [5], such as nitrate, sulfate, chloride and acetate, and heterogeneous processes on cobalt oxides and supported composites [6,7,8], have been explored in succession. Subsequently, metal-free carbocatalysis [9,10,11,12,13]—studied mainly by Wang and Sun’s group—attracted great attention compared to metal heterogeneous catalysts. Even though other transition metals (Mn, Cu, Zn, Ni etc.) [14] were also effective in PMS activation, the cobalt system with no need for activity-enhancing assistance (such as microwave, UV, visible light, thermal activation, etc.) was the most popular choice for investigation. Iron possesses the advantages of low cost, rich supplies and environmental friendliness, so it has been widely applied in water remediation. The addition of Fe into the cobalt compound can not only enhance the reactivity of PMS activation through enriching hydroxyl groups on the surface, but also endow the catalyst with easier separation and recovery properties due to its magnetism, as well as suppressing cobalt leaching owing to the strong Co-Fe interactions [15]. Hu et al. prepared the catalyst by one-step incipient wetness impregnation and put forward that in comparison with Co/SBA-15, CoFe/SBA-15 maintained higher catalytic activity and better stability, and its recovery was also more easily accomplished. Iron-cobalt oxide catalysts coupled with PMS have been reported to be efficient in organics degradation [16]. More recently, octahedral CoFe/CoFe2O4 was synthesized using a one-pot hydrothermal method and displayed excellent PMS activity [17]. Different series of Co-Fe oxides were prepared by thermal oxidation [15], sol-gel [18], co-precipitation [19,20], hydrothermal [21] and precipitation-oxidation [22] methods, with their application areas including PMS activated pollutant degradation and adsorption processes.
Previously, our group synthesized TiO2 and metal-doped TiO2 through a soft chemical solution process, which exhibited good photocatalytic activity in Methylene Blue (MB) degradation [23,24,25]. Afterwards, zinc ferrite was obtained through the same method and showed good photo-Fenton-like activity in Orange II degradation by PMS activation under visible light irradiation [26]. With the aim of avoiding the energy-consuming usage of visible light, we set out to fabricate a highly active cobalt-iron catalyst through such a soft chemical solution process. In the frame of this study, for the first time, a series of cobalt-iron catalysts including CoFe2O4 spinel, Co-Fe alloy and Co-Fe nitride, were prepared through soft chemical solution method followed by calcination under different atmospheres (air, N2 and NH3). The catalytic performances of the corresponding catalysts were investigated in PMS catalytic activation for Orange II degradation, which displayed high efficiency in organics treatments. Most importantly, Co-Fe nitride was found to have good activity and excellent stability in catalytic activation of PMS for dye degradation for the first time.

2. Results and Discussion

2.1. Basic Characterization of Cobalt-Iron Catalysts

The crystalline structures of the synthesized cobalt-iron catalysts were determined by XRD technique. Based on the XRD patterns (Figure 1), all the diffraction peaks of CFA-500 (referring to cobalt-iron catalyst calcined under air at 500 °C) and CFA-600 (referring to cobalt-iron catalyst calcined under air at 600 °C) can be attributed to CoFe2O4 spinel ferrite (JCPDS 00-022-1086). For the CFN samples (referring to cobalt-iron catalysts calcined under N2), distinct peaks at 2θ values of 44.8° (110) and 65.3° (200) can be indexed to Co-Fe alloy (Wairauite, JCPDS 00-044-1433). When calcined under ammonia, the main diffraction peaks at 37.5, 40.9, 42.9, 56.7, 67.7 and 75.9° were assigned to Co-Fe nitride (having a crystal structure analogous to that of Fe2N, JCPDS 01-072-2126) for CFNH-600 (referring to cobalt-iron catalyst calcined under ammonia at 600 °C). But CFNH-500 (referring to cobalt-iron catalyst calcined under ammonia at 500 °C) calcined at lower temperature still contained alloy beside the main nitride phase (having similar crystal structure to that of FeN0.09, JCPDS 01-075-2140) with low N content. Higher temperature promoted the formation of nitride phase. In addition, it was found that with the increase of the calcination temperature, the intensity of the diffraction peaks increased, indicating better crystallinity and larger particle size. According to the Scherrer equation, the grain size is 13.0, 41.7, 35.8 and 47.7 nm for CFA-500, CFA-600, CFN-500 (referring to cobalt-iron catalyst calcined under N2 at 500 °C), and CFN-600 (referring to cobalt-iron catalyst calcined under N2 at 600 °C), respectively. The nitride grain size is about 18.2 nm in the CFNH-500 sample while the Co-Fe alloy has grain size of about 30 nm. The main nitride phase of CFNH-600 gives grain size of 24 nm calculated from its (011) crystal plane. It can be deduced that the crystal structure of the prepared cobalt-iron catalysts mainly depends on the calcination atmosphere. Phase-pure samples of cobalt-iron oxide, alloy and nitride were obtained by calcination at 600 °C, which were chosen as catalysts for performance evaluation as discussed below.
The morphologies presented by SEM for the prepared Co/Fe-based catalysts are shown in Figure 2. Obviously, the air-calcined sample of CFA-500 exhibited sphere-like nanoparticles with the size of 10–20 nm (Figure 2a), which was consistent with the XRD results. Increasing the calcination temperature led to particle aggregation (Figure 2b). When the calcination was conducted in a nitrogen atmosphere, the resultant CFN samples exhibited bright, highly dispersed sphere-like nanoparticles representing the Co-Fe alloys, along with some petal-like layers on the surface (Figure 2c,d). According to the element analysis, the distinctive morphology on the surface of CFN-500 and CFN-600 could be attributed to the formation of cobalt-iron oxide resulting from the slight surface oxidation during the passivation process, which is consistent with the Mössbauer results below. With the increase of calcination temperature, the particles tended to grow larger. Relatively large nanoparticles with irregular shape can be found in CFNH-500 (Figure 2e), while an increase of the calcination temperature up to 600 °C resulted in a clearly different morphology. Namely, in the latter case, severe sintering took place accompanied by formation of little porous structure (Figure 2f). It is worth mentioning that N was successfully introduced into the samples during the calcination process, with its concentration increasing from 23% to 34% with the increase of temperature according to the energy spectrum analysis results. Correspondingly, the relative contents of Co and Fe increased but those of C and O decreased with increasing temperature. The SEM images demonstrated that different kinds of morphologies were developed under different calcination atmospheres.
TEM images of the obtained samples are presented in Figure 3. The particle size characteristic of CFA-500 was ~10 nm (Figure 3a), and about 40 nm for CFA-600 (Figure 3b) showing that the higher calcination temperature promoted the formation of larger particles, in agreement with corresponding SEM and XRD results. Nevertheless, metal particles dispersed on carbon support were obtained by N2 calcination (Figure 3c,d). Carbon in CFN samples is generated from the carbonization of organic species present in reactants during calcination under nitrogen. One can discern that many dark-colored nanoparticles (metal species) were dispersed in the light-colored matrix, which was ascribed to carbon species formed during the carbonization process. The nanoparticles grew larger, even to 50 nm, when the calcination temperature was increased from 500 to 600 °C. As for the CFNH-500, non-uniform nanoparticles were observed, interestingly, with the appearance of a core-shell structure (Figure 3e). However, irregular morphology was present on the Co-Fe nitride (Figure 3f). It is clear that higher calcination temperature leads to severe particle aggregation and larger particle sizes.
Figure 4 displays the N2 adsorption-desorption isotherms and corresponding pore size distribution of the prepared Co/Fe-based catalysts. Corresponding textural parameters are displayed in Table S1. Except CFNH-600, other samples give isotherms with hysteresis loops at relatively high pressures of 0.4–1.0, which indicates the existence of mesopores generated due to the accumulation of nanoparticles. This is confirmed by the calculated pore size distribution that exhibits mesopores (mainly in the range of 2–40 nm), and some macropores (>50 nm) as well. The absence of accumulation pores in CFNH-600 can be attributed to its bulk particles, which were generated via aggregation during calcination. The large particle size of CFNH-600 also leads to its lower BET surface area (13.0 m2 g−1) and pore volume (0.019 cm3 g−1) relative to other samples. Regardless of the calcination atmosphere, with the increase of calcination temperature, the BET specific surface area and pore volume decrease markedly for all the samples, which is another consequence of the particle aggregation, in accordance with SEM and TEM results. The large surface area of the N2-calcined samples, especially for CFN-500, is mainly due to the existence of carbon in samples.

2.2. 57Fe Mössbauer Spectroscopy Characterization

Mössbauer spectroscopy is an excellent tool for examining the local environment of Fe in cobalt-iron catalysts. Room temperature 57Fe Mössbauer spectra of the six samples are shown in Figure 5a–f, together with their fit. In the case of CFA-500 and CFA-600, the spectra (Figure 5a,b) mainly reflect the presence of Fe3+ in the CoFe2O4 spinel phase with a partial degree of inversion. CoFe2O4 is known to prefer a partially inverse spinel structure where majority of the A (tetrahedral) site is taken by Fe3+ [27,28]. We can observe three components corresponding to Fe3+ in tetrahedral (A) site (sextet), octahedral (B) site (sextet with broad peaks reflecting binomial distribution of cobalt atoms at the tetrahedral site) and the smallest particles with superparamagnetic nature (quadrupole doublet). There is a more complete level of inversion (i.e., a lower concentration of Co at tetrahedral sites) present in the sample CFA-600, than in CFA-500, which is presumably connected to the higher calcination temperature applied in the former case. A less intense Fe3+ doublet component, accounting for less than 1% of the spectral area, may also be present in the spectra (Table S2). Its contribution is smaller in the case of CFA-600, suggesting that higher calcination temperature and/or higher particle size tends to diminish its presence.
In case of samples CFN-500 and CFN-600, the spectra (Figure 5c,d) indicate the presence of the bcc FexCo1−x alloy phase with an Fe:Co ratio that is close to 2:1 in both cases (The fit of the corresponding component was carried out as described in the previous work [29]). A heavily broadened spectral component can be seen in CFN-500 as being associated with the smallest Co-Fe alloy particles that undergo magnetic relaxation on a time scale which is comparable to the Larmor precession time of the 57Fe nucleus. This component is missing from the spectrum of CFN-600 (Figure 5d), in agreement with the larger characteristic particle size of the latter sample. A paramagnetic Fe3+ doublet component can also be detected in the spectrum of these samples, with a considerably smaller relative spectral area for CFN-600 (~2%) than for CFN-500 (~7%) (Table S3), suggesting that this amount can be reduced by increasing the calcination temperature.
In the sample that was calcined at 500 °C under NH3 atmosphere, one can detect both Co-Fe alloy (magnetic sextet component) and Co-Fe nitride (paramagnetic doublet components) (Figure 5e, Table S4). In contrast, only one paramagnetic iron doublet is observed (Figure 5f) when the calcination was carried out at 600 °C: the Mössbauer parameters of the doublet are similar to those of Fe2N [30], which is consistent with the XRD results.

2.3. Surface Elements Analysis

XPS measurements were carried out on the cobalt-iron samples to investigate the surface characteristics. Full XPS survey in Figure 6a shows the compositional information of the sample CFA-600, indicating the presence of Co, Fe, O, as well as C. The high-resolution XPS spectra of Co 2p, Fe 2p and O 1s are shown in Figure 6b–d, respectively. The Co 2p3/2 peaks at 779.5 eV and 781.5 eV were ascribed to Co2+ at octahedral (B) and tetrahedral (A) sites of the spinel structure, respectively, with a satellite peak of Co 2p3/2 at ~785.5 eV [31]. There were also two peak signals for Fe 2p3/2 at 710.0 and 712.7 eV, suggesting the occupation of octahedral and tetrahedral sites, respectively. Additionally, one satellite peak appeared at 719.1 eV, which was further proof for the existence of Fe3+. The O 1s peaks at 529.5 and 531.1 eV were assigned to lattice oxygen and surface adsorbed oxygen, respectively. The results are consistent with the Mössbauer fit results that spinel structured cobalt ferrite with some degree of inversion was observed. Similar spectra were obtained on the sample CFA-500 (Figure S1), revealing that the main phase of samples obtained under air was cobalt ferrite.
XPS of CFN samples were also studied, as shown in Figure S2 and Figure 7. Due to the limited penetration depth (less than 10 nm), XPS analysis reflects only surface composition characteristics. Thus, although the XRD patterns suggested the presence of significant amounts of Co-Fe alloy, the metal concentrations of Co and Fe on the surface were so low that we cannot observe corresponding strong XPS signals on CFN-500, as reflected by the low detected Co and Fe atomic contents of 0.32% and 0.55%, respectively. Carbon was the main species on the surface of CFN-500 and CFN-600. A broad C1s peak suggested four different C species in CFN-500 (Figure S2) in the range of 283–290 eV. The peaks at 284.5, 285.5, 286.5 and 288.3 eV were assigned to C=C (or C–C), C–O, C=O or O–C–O and O–C=O, respectively [32]. However, the Co 2p and Fe 2p peaks could be distinguished evidently on CFN-600 (Figure 7), maybe because of the relatively higher contents of Co (2.86%) and Fe (3.87%) on the surface. The Co 2p3/2 peaks at 778.2 and 781.1 eV were ascribed to Co0 and Co2+, respectively, with a satellite peak at 786.6 eV. As for iron, beside Fe3+, a small amount of Fe0 can be observed through the peak of 708.1 eV [17]. Thus, we can discern that the metals on the surface were oxidized by the ambient air to some extent. Furthermore, only three peaks at about 284.6, 285.4 and 286.2 eV were observed showing a dramatic decrease in carbon-bonded oxygen groups along with the absence of carboxyl group. The results indicate that the carbon species obtained at different carbonization temperatures display different characteristics. In order to illustrate the variation between the CFN-500 and CFN-600, thermal analysis under inert atmosphere with a heating rate of 10 °C min−1 was conducted, as shown in Figure S3a. The TGA plots revealed dramatic weight loss from 200 to 600 °C, which can be assigned to the removal or destruction of oxygenated functional groups. Two main endothermic peaks can be observed at about 300 and 530 °C, accompanied by the release of CO and CO2 as determined with TG-MS technique (Figure S3b), suggesting that carbonization occurred and two different carbon-containing complexes were decomposed during these processes. The appearance of CO indicated that self-reduction occurred during the calcination, resulting in the formation of Co-Fe alloy. Importantly, the second endothermal peak appeared at about 533 °C, clearly revealing that the reducing degree under 600 °C was higher than that of 500 °C and that different carbon-bonded groups were found in CFN-500 and CFN-600.
Chemical states of surface elements in cobalt-iron nanomaterials CFNH-500 and CFNH-600 obtained under ammonia atmosphere are presented in Figure S4 and Figure 8, respectively. From the survey in Figure 8a, clear peaks of Co, Fe, C, N and O were observed, further certifying the successful introduction of element N through NH3 calcination. High resolution Co 2p3/2 peaks present at 780.4 and 782.7 eV can be ascribed to Co2+ and Co3+, respectively, with a satellite at 786.6 eV (Figure 8b). Concerning iron, only Fe3+ was detected with a satellite peak at 719.1 eV (Figure 8c). However, peaks of 778.5 and 707.9 eV were also found in the case of CFNH-500 (Figure S4), which can be assigned to metallic Co0 and Fe0, consistent with the XRD result that Co-Fe alloy was formed under 500 °C. The appearance of high valence cobalt and iron suggested that the surface of the sample was oxidized when exposed to air, similarly to the case of the CFN samples. In addition to Co and Fe, high resolution XPS peaks of C, N and O were also observed. Peaks centered at 284.6, 285.8, 286.9 and 288.6 eV (Figure 8d) can be attributed to the C=C or C–C, C–O or C–N, C=O and O–C=O, respectively [33,34]. The N1s spectrum (Figure 8e) can be deconvoluted into five peaks centered at 397, 398.6, 400.1, 402.7 and 404.7 eV, representing different kinds of nitrogen species and confirming the presence of N in the sample. The peaks at 397, 400.1, 402.7 and 404.7 eV could be assigned to the pyridinic, pyrrollic, graphitic N and oxidized pyridinic N [35,36]. The peak at 398.6 eV was ascribed to the pyridinic N coordinated with Fe or Co, i.e., N–Fe or N–Co, according to the literatures [36,37]. Less than 10% of graphitic N was found. The majority of pyridinic N resulting from the coordination with metal (Fe or Co) [38], verified the formation of metal nitride. The O 1s peaks at 530.0 and 531.7 eV (Figure 8f) were ascribed to the lattice oxygen coordinated with metal and surface hydroxyl oxygen, respectively [39]. It should be noted that a peak at 536.0 eV, which may originate from organics residuals such as carboxyl groups, was also detected for both CFNH-500 and CFNH-600.

2.4. Catalytic Degradation of Orange II Solutions

In order to recognize and clarify the PMS activation performance of different types of Co/Fe-based catalysts (i.e., oxide, alloy and nitride), the samples calcined at 600 °C under different atmospheres were chosen to catalyze PMS activation for Orange II degradation. According to Figure 9A, no degradation can be obtained during the tested time if there are no catalysts in the system (curve a), suggesting the important role of catalysts. The catalysts cannot provide obvious removal of Orange II without PMS (see from the adsorption stage of 30 min before zero point of x axis), suggesting that the contribution from adsorption could be negligible. Noticeably, there was about 10% dye removal on the CFN-600, which may have resulted from the existence of carbon. After PMS addition, the removal rate of Orange II on the catalysts calcined under N2 (CFN-600) was significantly higher than that of CFA-600 and CFNH-600. CFN-600 was able to effectively degrade Orange II through activating PMS to produce oxidizing species, with more than 90% removal within 10 min. For the CFNH-600, whose catalytic performance was evidently inferior to CFN-600, 80 min was needed to realize the same efficiency. However, the removal rate was less than 50% even at the time of 90 min on CFA-600, suggesting that the cobalt ferrite exhibited the lowest activity among the three kinds of Co-Fe catalysts. The superior activity of Co-Fe alloy may be a result mainly of the higher reduction ability of the zero valent metal. Besides, according to the ICP results (Table S5), Co-Fe alloy gave more metal ions leaching, which could also contribute to the degradation activity through homogeneous catalysis. In comparison to the spinel, the nitride catalyst displayed superior activity in PMS activation, which may be due to the different adsorption surfaces with PMS molecules endowing the nitride with stronger adsorption energy, longer O-O bond lengths and more transferred electrons [40]. On the whole, according to the activity measurements the Co-Fe alloy provided the highest Orange II removal efficiency and the activity order of the different catalysts is CFN-600 > CFNH-600 > CFA-600.
In order to estimate the kinetic parameter of the degradation reactions, first order kinetics was employed for PMS activated pollutant degradation, with the equation
ln ( c 0 c ) = k t
where k is the apparent first order rate constant of Orange II removal, c0 is the original concentration of Orange II aqueous solution, c is the real time concentration of Orange II during the reaction, and t is the reaction time. The reaction rate constants (Figure 9B) for CFA-600, CFN-600 and CFNH-600 were estimated to be 0.007 (R2 = 0.976), 0.322 (R2 = 0.939) and 0.024 (R2 = 0.907) min1, respectively. Based on the appropriate regression coefficients for the reaction system, the pseudo-first-order kinetic was basically thought to fit well with the experiment. These catalysts yielded results that were similar to those of the previous studies [41,42], where the kinetic rate of organic pollutants was explored in the presence of PMS. The rate constant of CFN-600 was 46 times and 13.4 times higher than that of the CFA-600 and CFNH-600 samples, respectively, suggesting the excellent performance of the Co/Fe-based catalysts obtained under N2 atmosphere. The catalytic efficiency of Co-Fe nitride was 3.4 times better than the corresponding CoFe2O4 in this study, clearly revealing the superiority of nitride. The sequence of the catalytic activity of different types of cobalt-iron samples is Co-Fe alloy > Co-Fe nitride > Co-Fe oxide.
Apart from the excellent catalytic activity, the stability and reusability of a heterogeneous catalyst is also crucial in the catalytic reaction processes. Figure 10 shows the successive test results of the three cobalt-iron catalysts calcined at 600 °C for Orange II degradation. It can be seen that deactivation took place on the spinel and alloy catalysts during the measured time (Figure 10a,b). At the same time, the nitride kept the original activity, indicating its high stability and reusability (Figure 10c). Previous literature made the point that the formation of Fe3C contributed to a better stability in the Fe0/Fe3C@CS catalyst [43]; in our case, nitride may play a similar role. Besides, manganese nitride (Mn4N) was reported to possess good stability compared to the zero valent Co, Fe and Mn in PMS activation for BPA degradation [40]. From the point of view of reusability and stability, Co-Fe nitride exhibited the best performance. According to the XRD patterns (Figure S5) of the used cobalt-iron catalysts, no variation took place in the phase composition compared to the fresh catalysts. However, surface chemical compositions and states of the used catalysts experienced partial oxidation for CFA-600 and CFN-600. In the used CFA-600, a new peak appeared at 783.1 eV representing Co3+ in octahedral site appeared (Figure 11a), indicating the oxidation of Co2+ to Co3+ during the catalytic reaction. This transformation was also reported by Ren et al. who found that Co3+ emerged after PMS activated degradation [18]. Besides, no significant variation took place in the valence state of Fe before and after reaction, since only Fe3+ was observed (Figure 11b). As for CFN-600, the peak of Co0 disappeared, at the same time, the peak at 783.3 eV representing Co3+ turned up compared to the fresh catalyst (Figure 11c). It was demonstrated that metallic Co0 was totally oxidized, and Co2+ was partially oxidized into Co3+ during the catalytic oxidation reaction. Concerning iron, only Fe3+ was present in the used catalyst (Figure 11d), manifesting the oxidation of metallic Fe0. It was found that Fe0 was reactive in catalytic PMS activation, being converted to Fe(II)/Fe(III) after the reaction [43,44]. These results demonstrated that the active species on the catalyst surface were oxidized to some extent, which was one of the proofs for the deactivation. Besides, according to the XPS results in Figure S6, element sulfur was discovered for the used CFN-600 sample, suggesting that organic compounds were adsorbed on the catalysts, which could be another reason for its deactivation. From the adsorption curves in Figure 10b, the adsorbed amounts of Orange II decreased from run1 to run3, suggesting the decreased adsorption ability and the coverage of the catalyst surface. More importantly, after extending the reaction time to 80 min (Figure 10d), the CFN-600 sample presented good reusability with no deactivation in run2 and run3, further verifying that adsorbed organics were the main reason for the deactivation testing in a short time (Figure 10b). Thus, surface active sites may be covered by the adsorbed organic compounds during reaction, resulting in the decrease of activity. Similar results were obtained on the CFNH-600 sample (Figure 12a), where sulfur was detected only after reaction. But the small BET surface area of the nitride sample may inhibit the adsorption of organic species from having appreciable impact on the activity of the catalyst, endowing it with better reusability. No significant changes were found on the variation of total pyridinic N (59 ± 2%), pyrrolic N (25 ± 2%), graphitic N (10 ± 2%) and oxidized nitrogen species (5 ± 1%) in the fresh and used catalyst (Table S6), certifying the superior stability of nitrides.
To explore the variation in the chemical state of Fe, 57Fe Mössbauer spectra of the used catalysts were also measured, as shown in Figure 13. For CFA-600, there was no appreciable change detected concerning the Fe3+ species in the spinel, but the relative area fraction of the paramagnetic Fe3+ doublet component increased up to ~2.5% (Table S2). Similarly, the paramagnetic Fe3+ doublet in CFN-600 increased from ~2% to 9% during reaction (Table S3), with a corresponding decrease in metallic Fe0 in the Co-Fe alloy phase, which also refers to the oxidation of catalysts, in agreement with the XPS results. No variation occurred in the state of Fe in CFNH-600, providing further confirmation in the stability of this catalyst. Hence, the good stability and reusability made the nitride more promising in the environmental remediation.

2.5. Reaction Mechanism Study

Previous investigations have pointed out that in the cobalt-iron homogeneous and heterogeneous catalytic activation of the peroxymonosulfate reaction, sulfate radical (SO4·−) and hydroxyl radical (·OH) can always be identified as the main reactive species [45]. To ascertain the main intermediate active species in the three different systems, radical scavenger tests were taken in this study. It is widely accepted that alcohols with an α-hydrogen such as ethanol readily react with both SO4·− and ·OH (1.6–7.7 × 107 M−1 s−1 and 1.2–2.8 × 109 M−1 s−1, respectively), while those without α-H, such as tert-butyl alcohol (TBA), react more easily with ·OH (3.8–7.6 × 108 M−1 s−1), but in a much more slower reaction rate with SO4·− (4.0–9.1 × 105 M−1 s−1) [46,47]. Thus, TBA as a particular scavenger for ·OH and ethanol as a universal scavenger for both SO4·− and ·OH were used to differentiate the contribution of SO4·− from ·OH. In the organic degradation process, where radicals played a decisive role when the quenching agent was added into the solution, the degradation would be either prevented or significantly reduced. As shown in Figure 14, degradation was inhibited for all three samples with the addition of ethanol. More importantly, there was hardly any effect observed on the CFN-600 sample when using the same amounts of TBA as a scavenger, suggesting that sulfate radical was the main reactive species. As for CFA-600 and CFNH-600, the addition of TBA caused some inhibiting effects in the Orange II degradation efficiency, but ethanol made a more significant contribution. Therefore, we could conclude that sulfate radical played the key role in the CFA-600/PMS and CFNH-600/PMS systems, with a certain amount of hydroxyl radical; only sulfate radical played a role as reactive species in the CFN-600/PMS system.
In the past years, several investigations have been carried out to recognize the mechanism of Co/Fe-based catalysts in the activation of PMS. It has been reported that when CoFe2O4 was used as a catalyst for PMS activation, cobalt mainly presented as Co2+ before reaction, and it underwent partial transformation to Co3+ after catalytic reaction, in which the involvement of Co2+-Co3+-Co2+ redox processes were proposed during the reaction [18]. In addition, sulfate radical was found to be generated as the main active species in oxone activation by cobalt-iron oxides [22,48]. Concerning the CFA sample in the present study, the reaction mechanism for Orange II degradation can be proposed as following (Equations (2)~(7)).
≡Co2+ + HSO5 → ≡Co3+ + SO4·− + OH
≡Fe2+ + HSO5 → ≡Fe3+ + SO4·− + OH
≡Co3+ + HSO5 → ≡Co2+ + SO5·− + H+
≡Fe3+ + HSO5 → ≡Fe2+ + SO5·− + H+
≡Fe2+ + ≡Co3+ → ≡Co2+ + ≡Fe3+
SO4·− + Orange II → many steps → CO2 + H2O + SO42
It was reported that the active sites are mainly the cobalt and iron ions in the spinel type CoFe2O4 and the zero-valent cobalt and iron for the octahedral CoFe/CoFe2O4 submicron composite [17]. In the case of the CFN sample, the following reactions (Equations (8)~(11)) may be considered, with the rest of the steps being identical to processes described by Equations (2)~(7) above.
≡Co0 + 2HSO5 → ≡Co2+ + 2SO4·− + 2OH
≡Fe0 + 2HSO5 → ≡Fe2+ + 3SO4·− + 2OH
≡Co0 + 2≡Co3+ → 3≡Co2+
≡Fe0 + 2≡Fe3+ → 3≡Fe2+
For the Co-Fe nitride, the redox process of Co2+-Co3+-Co2+ also exist in the system, and one can observe only small changes in the relative amounts of Co2+ and Co3+ according to the XPS fitting results of the CFNH-600 before and after reaction. The potential mechanism could be speculated to be similar to that mentioned for the CFA sample, except that the introduction of N into the catalyst made its stability appreciable, and at the same time, the activity superior to the oxide.

3. Materials and Methods

3.1. Chemicals

Cobalt acetylacetonate (Co(acac)2), ferric acetylacetonate ((Fe(acac)3), Orange II sodium salt (C16H11N2NaO4S) and tert-butyl alcohol (TBA, >99.5%) were purchased from Aladdin Chemistry Co. Ltd. (Shanghai, China) 2-ethoxyethanol (C4H10O2) and methanol (CH3OH, ≥99.5%) were purchased from Tianjin Damao Chemical Reagent Company (Tianjin, China) and H2O2 (30 wt.%) from Tianjin Kermel Chemical Reagent Company (Tianjin, China). PMS was purchased from Alfa Aesar (Tianjin, China). Ethanol (CH3CH2OH, ≥99.7%) was obtained from Sinopharm Chemical Reagent Co. Ltd. (Shanghai, China). All the chemicals were analytical grade with no further treatment. Deionized water was used for solution preparation.

3.2. Synthesis of Cobalt-Iron Catalysts

Co/Fe-based catalysts were prepared through an extended soft chemical solution process reported previously [49,50]. Typically, Co(acac)2 and Fe(acac)3 (molar ratio 1:2) were first dissolved homogeneously together in 50 mL 2-ethoxyethanol within 1 L beaker at 50 °C, followed by slow addition of 30 mL H2O2 aqueous solution under magnetic stirring. The suspension was obtained after rotary evaporation and drying. Finally, the catalysts were obtained by calcining the solid precursors at 500 or 600 °C under special atmosphere. The prepared cobalt ferrite samples are denoted as CFX-T, where X represents the calcination atmosphere of air (A), nitrogen (N) and ammonia (NH) and T represents the final calcination temperature.

3.3. Catalysts Characterization

The X-ray diffraction (XRD) patterns were measured on a PW3040/60 X’Pert PRO diffractometer (PANalytical, Alemlo, The Netherlands) equipped with a copper target (Cu Kα radiation, λ = 1.5406 Å) at an accelerating voltage of 40 kV, a current of 40 mA, and a scanning 2θ range of 10°–80° at room temperature. The average crystallite sizes were calculated by Scherrer equation as below:
φ = K λ β c o s θ
where φ is the average crystallite size, K is the Scherrer constant (taken to be equal to 0.89); λ is the wavelength of the used X-ray, θ is the diffraction angle of the calculated peak, and β is the full width at half maximum height (FWHM) of the mean intensity peak. The morphological feature was observed on a JEM-2000EX electronic microscope (JEOL, Tokyo, Japan) with an accelerating voltage of 120.0 kV. The sample was dispersed in the ethanol solution and then withdrawn to drop on a copper grid for measurement. The field-emission scanning electron microscopy (FESEM, JSM-7800F) (JEOL, Tokyo, Japan) was operated at an accelerating voltage of 3.0 kV, and the sample was put onto a conductive carbon tape to be measured. Textural information was measured by nitrogen adsorption/desorption at 77 K using a Micromeritics ASAP 2460 apparatus (Micromeritics, Norcross, GA, USA). Prior to measurement, all the samples were pretreated in vacuum at 110 °C for 1 h, followed by 300 °C for 6 h. The thermogravimetric and differential scanning calorimetry (TG-DSC) curves in N2 were investigated on a TGA instrument Q600 (TA, New Castle, PA, USA) with alumina crucible as sample holder, and the heating rate was set at 10 °C min−1 with flow rate of 100 mL min−1. The metal ion leaching amount after reaction was determined by inductively coupled plasma-atomic emission spectrometry (ICP-AES) on an IRIS Intrepid II XSP instrument (rThermoFisher, Waltham, MA, USA). The X-ray photoelectron spectroscopy (XPS) experiment was performed on an ESCALAB250 X-ray photoelectron spectrometer (ThermoFisher, Waltham, MA, USA) with monochromatic Al Kα as the X-ray source, and contaminated carbon was used as the internal standard (C1s = 284.6 eV). 57Fe Mössbauer spectra were measured on a Topologic 500A spectrometer employing a 57Co(Rh) as γ-ray radioactive source moving in a constant acceleration mode at room temperature. The spectra were fitted by using the MossWinn 4.0 program [51]. Room temperature α-iron foil was applied for the calibration of the velocity axis, and 57Fe isomer shift values are quoted relative to that of the standard.

3.4. Activity Evaluation

The prepared cobalt-iron catalysts were applied in catalytic degradation of Orange II by activation of PMS. All the experiments were carried out in a beaker with constant rotation speed. Prior to the degradation experiments, proper amounts of catalyst were mixed with Orange II solution under stirring for 30 min to achieve adsorption-desorption equilibrium, and then PMS was added into the system to initiate the reaction. The typical concentrations of catalyst, PMS and Orange II were 0.1 g L−1, 0.5 g L−1 and 50 mg L−1, respectively. At certain time intervals, 1 mL reaction solution was withdrawn and quenched immediately by adding 1 mL methanol solution. After centrifugation, the supernatant was analyzed by the GBC Cintra apparatus to record variation of the absorption peak intensity (wavelength at 484 nm for Orange II aqueous solution).

4. Conclusions

Three kinds of cobalt-iron catalysts with the dominant phase of CoFe2O4 spinel, Co-Fe alloy and Co-Fe nitride were successfully synthesized through extended soft chemical solution processes followed by atmosphere-dependent calcination. All these obtained catalysts were applied to the Orange II degradation by PMS activation and performed good pollutants removal efficiency. By comparison, Co-Fe alloy exhibited the best activity and Co-Fe nitride possessed very good stability. Sulfate radical was proved to be the main active species in Co-Fe alloy system, while hydroxyl radical is also effective in the Co-Fe nitride and CoFe2O4 participant reactions. Considering the severe leaching problem of the zero valent metals, efforts need to be made to retard the leaching problem and improve the stability. Besides, the detailed properties and mechanisms of the catalysts especially for the nitride-derived catalysts need to be further explored.

Supplementary Materials

The following are available online at www.mdpi.com/2073-4344/7/5/138/S1, Figure S1: XPS spectra of CFA-500 in different regions (a) survey, (b) C 1s, (c) Co 2p, (d) Fe 2p. Figure S2: XPS spectra of CFN-500 in different regions (a) survey, (b) Co 2p, (c) Fe 2p, and (d) C 1s.Figure S3: TG-DSC (a) and the TG-MS (b) curves of the as-prepared cobalt-iron nanomaterials under Ar atmosphere. Figure S4: XPS spectra of CFNH-500 in different regions (a) survey, (b) Co 2p, (c) Fe 2p, (d) C 1s, (e) N 1s and (f) O 1s. Figure S5: XRD patterns of the used CFA-600, CFN-600 and CFNH-600. Figure S6: S2p XPS spectrum of the CFN-600 before and after reaction. Table S1: The BET surface area and pore volume of prepared samples. Table S2: 57Fe Mössbauer parameters of the samples CFA-500 and CFA-600 as well as CFA-600-after reaction derived on the basis of Mössbauer spectra recorded at room temperature. Table S3: 57Fe Mössbauer parameters of the samples CFN-500 and CFN-600 as well as CFN-600-after reaction derived on the basis of Mössbauer spectra recorded at room temperature. Table S4: 57Fe Mössbauer parameters of the samples CFNH-500 and CFNH-600 derived on the basis of Mössbauer spectra recorded at room temperature. Table S5: Metal leaching concentrations detected by ICP. Table S6: XPS fitting results of surface elements for the CFA-600, CFN-600 and CFNH-600 samples before and after reaction.

Acknowledgments

This work was supported by the National Natural Science Foundation of China [grant numbers 21476232, 21403220, 2161101071], China Ministry of Science and Technology [grant number 2016YFA0202804] and the CAS President’s International Fellowship Initiative (PIFI) program for a postdoctoral researcher funded by the Chinese Academy of Sciences [grant number 2016PT023].

Author Contributions

K.Z. and J.W. conceived and designed the experiments; K.Z. performed the experiments; K.Z. C.J. and Z.K. analyzed the data; K.Z. wrote the paper; A.S.G. contributed to the data analysis and paper revision.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Cizmas, L.; Sharma, V.K.; Gray, C.M.; McDonald, T.J. Pharmaceuticals and personal care products in waters: Occurrence, toxicity, and risk. Environ. Chem. Lett. 2015, 13, 381–394. [Google Scholar] [CrossRef]
  2. Cheng, M.; Zeng, G.; Huang, D.; Lai, C.; Xu, P.; Zhang, C.; Liu, Y. Hydroxyl radicals based advanced oxidation processes (AOPs) for remediation of soils contaminated with organic compounds: A review. Chem. Eng. J. 2016, 284, 582–598. [Google Scholar] [CrossRef]
  3. Zhang, B.T.; Zhang, Y.; Teng, Y.H.; Fan, M.H. Sulfate radical and its application in decontamination technologies. Crit. Rev. Envrion. Sci. Technol. 2015, 45, 1756–1800. [Google Scholar] [CrossRef]
  4. Hu, P.; Long, M. Cobalt-catalyzed sulfate radical-based advanced oxidation: A review on heterogeneous catalysts and applications. Appl. Catal. B 2016, 181, 103–117. [Google Scholar] [CrossRef]
  5. Chan, K.H.; Chu, W. Degradation of atrazine by cobalt-mediated activation of peroxymonosulfate: Different cobalt counteranions in homogenous process and cobalt oxide catalysts in photolytic heterogeneous process. Water Res. 2009, 43, 2513–2521. [Google Scholar] [CrossRef] [PubMed]
  6. Qi, F.; Chu, W.; Xu, B.B. Modeling the heterogeneous peroxymonosulfate/Co-MCM41 process for the degradation of caffeine and the study of influence of cobalt sources. Chem. Eng. J. 2014, 235, 10–18. [Google Scholar] [CrossRef]
  7. Cai, C.; Zhang, H.; Zhong, X.; Hou, L.W. Ultrasound enhanced heterogeneous activation of peroxymonosulfate by a bimetallic Fe-Co/SBA-15 catalyst for the degradation of orange II in water. J. Hazard. Mater. 2015, 283, 70–79. [Google Scholar] [CrossRef] [PubMed]
  8. Zhou, G.; Zhou, L.; Sun, H.; Ang, H.M.; Tadé, M.O.; Wang, S. Carbon microspheres supported cobalt catalysts for phenol oxidation with peroxymonosulfate. Chem. Eng. Res. Des. 2015, 101, 15–21. [Google Scholar] [CrossRef]
  9. Duan, X.; Ao, Z.; Sun, H.; Zhou, L.; Wang, G.; Wang, S. Insights into N-doping in single-walled carbon nanotubes for enhanced activation of superoxides: A mechanistic study. Chem. Commun. 2015, 51, 15249–15252. [Google Scholar] [CrossRef] [PubMed]
  10. Duan, X.; Ao, Z.; Zhou, L.; Sun, H.; Wang, G.; Wang, S. Occurrence of radical and nonradical pathways from carbocatalysts for aqueous and nonaqueous catalytic oxidation. Appl. Catal. B 2016, 188, 98–105. [Google Scholar] [CrossRef]
  11. Duan, X.; O’Donnell, K.; Sun, H.; Wang, Y.; Wang, S. Sulfur and nitrogen co-doped graphene for metal-free catalytic oxidation reactions. Small 2015, 11, 3036–3044. [Google Scholar] [CrossRef] [PubMed]
  12. Duan, X.; Sun, H.; Ao, Z.; Zhou, L.; Wang, G.; Wang, S. Unveiling the active sites of graphene-catalyzed peroxymonosulfate activation. Carbon 2016, 107, 371–378. [Google Scholar] [CrossRef]
  13. Sun, H.Q.; Liu, S.Z.; Zhou, G.L.; Ang, H.M.; Tade, M.O.; Wang, S.B. Reduced graphene oxide for catalytic oxidation of aqueous organic pollutants. ACS Appl. Mater. Interfaces 2012, 4, 5466–5471. [Google Scholar] [CrossRef] [PubMed]
  14. Sharma, R.; Kumar, V.; Bansal, S.; Singhal, S. Assortment of magnetic nanospinels for activation of distinct inorganic oxidants in photo-fenton’s process. J. Mol. Catal. A Chem. 2015, 402, 23–63. [Google Scholar] [CrossRef]
  15. Yang, Q.; Choi, H.; Al-Abed, S.R.; Dionysiou, D.D. Iron-cobalt mixed oxide nanocatalysts: Heterogeneous peroxymonosulfate activation, cobalt leaching, and ferromagnetic properties for environmental applications. Appl. Catal. B 2009, 88, 462–469. [Google Scholar] [CrossRef]
  16. Hu, L.X.; Yang, F.; Zou, L.P.; Yuan, H.; Hu, X. Fe/SBA-15 catalyst coupled with peroxymonosulfate for heterogeneous catalytic degradation of rhodamine B in water. Chin. J. Catal. 2015, 36, 1785–1797. [Google Scholar] [CrossRef]
  17. Sun, H.; Yang, X.; Zhao, L.; Xu, T.; Lian, J. One-pot hydrothermal synthesis of octahedral CoFe/CoFe2O4 submicron composite as heterogeneous catalysts with enhanced peroxymonosulfate activity. J. Mater. Chem. A 2016, 4, 9455–9465. [Google Scholar] [CrossRef]
  18. Ren, Y.M.; Lin, L.Q.; Ma, J.; Yang, J.; Feng, J.; Fan, Z.J. Sulfate radicals induced from peroxymonosulfate by magnetic ferrospinel MFe2O4 (M = Co, Cu, Mn and Zn) as heterogeneous catalysts in the water. Appl. Catal. B 2015, 165, 572–578. [Google Scholar] [CrossRef]
  19. Xu, L.J.; Chu, W.; Gan, L. Environmental application of graphene-based CoFe2O4 as an activator of peroxymonosulfate for the degradation of a plasticizer. Chem. Eng. J. 2015, 263, 435–443. [Google Scholar] [CrossRef]
  20. El-Shobaky, G.A.; Turky, A.M.; Mostafa, N.Y.; Mohamed, S.K. Effect of preparation conditions on physicochemical, surface and catalytic properties of cobalt ferrite prepared by coprecipitation. J. Alloys Compd. 2010, 493, 415–422. [Google Scholar] [CrossRef]
  21. Ding, Z.; Wang, W.; Zhang, Y.; Li, F.; Liu, J.P. Synthesis, characterization and adsorption capability for Congo Red of CoFe2O4 ferrite nanoparticles. J. Alloys Compd. 2015, 640, 362–370. [Google Scholar] [CrossRef]
  22. Wei, G.L.; Liang, X.L.; He, Z.S.; Liao, Y.S.; Xie, Z.Y.; Liu, P.; Ji, S.C.; He, H.P.; Li, D.Q.; Zhang, J. Heterogeneous activation of oxone by substituted magnetites Fe3-xMxO4 (Cr, Mn, Co, Ni) for degradation of acid orange II at neutral pH. J. Mol. Catal. A Chem. 2015, 398, 86–94. [Google Scholar] [CrossRef]
  23. Yu, F.H.; Wang, J.H.; Zhao, K.F.; Yin, J.; Jin, C.Z.; Liu, X. A novel approach for the preparation of phase-tunable TiO2 nanocomposite crystals with superior visible-light-driven photocatalytic activity. Chin. J. Catal. 2013, 34, 1216–1223. [Google Scholar] [CrossRef]
  24. Yu, F.; Wang, Y.; Tang, H.; Zhang, Y.; Jin, C.; Liu, X.; Li, M.; Wang, J. Synergic effect of cation doping and phase composition on the photocatalytic performance of TiO2 under visible light. Catal. Commun. 2014, 51, 46–52. [Google Scholar] [CrossRef]
  25. Wang, Y.; Zhang, Y.; Yu, F.; Jin, C.; Liu, X.; Ma, J.; Wang, Y.; Huang, Y.; Wang, J. Correlation investigation on the visible-light-driven photocatalytic activity and coordination structure of rutile Sn-Fe-TiO2 nanocrystallites for methylene blue degradation. Catal. Today 2015, 258, 112–119. [Google Scholar] [CrossRef]
  26. Zhu, K.; Wang, J.; Wang, Y.; Jin, C.; Ganeshraja, A.S. Visible-light-induced photocatalysis and peroxymonosulfate activation over ZnFe2O4 fine nanoparticles for degradation of orange II. Catal. Sci. Technol. 2016, 6, 2296–2304. [Google Scholar] [CrossRef]
  27. Sawatzky, G.A.; Van Der Woude, F.; Morrish, A.H. Cation distributions in octahedral and tetrahedral sites of the ferrimagnetic spinel CoFe2O4. J. Appl. Phys. 1968, 39, 1204–1206. [Google Scholar] [CrossRef]
  28. Le Trong, H.; Presmanes, L.; De Grave, E.; Barnabé, A.; Bonningue, C.; Tailhades, P. Mössbauer characterisations and magnetic properties of iron cobaltites CoxFe3−xO4 (1 ≤ x ≤ 2.46) before and after spinodal decomposition. J. Magn. Magn. Mater. 2013, 334, 66–73. [Google Scholar] [CrossRef]
  29. Klencsár, Z.; Németh, P.; Sándor, Z.; Horváth, T.; Sajó, I.E.; Mészáros, S.; Mantilla, J.; Coaquira, J.A.H.; Garg, V.K.; Kuzmann, E.; et al. Structure and magnetism of Fe–Co alloy nanoparticles. J. Alloys Compd. 2016, 674, 153–161. [Google Scholar] [CrossRef]
  30. Bainbridge, J.; Channing, D.A.; Whitlow, W.H.; Pendlebury, R.E. A Mössbauer and X-ray investigation of zeta Fe2N. J. Phys. Chem. Solids 1973, 34, 1579–1580. [Google Scholar] [CrossRef]
  31. Wang, W.P.; Yang, H.; Xian, T.; Jiang, J.L. Xps and magnetic properties of CoFe2O4 nanoparticles synthesized by a polyacrylamide gel route. Mater. Trans. 2012, 53, 1586–1589. [Google Scholar] [CrossRef]
  32. Indrawirawan, S.; Sun, H.; Duan, X.; Wang, S. Nanocarbons in different structural dimensions (0–3D) for phenol adsorption and metal-free catalytic oxidation. Appl. Catal. B 2015, 179, 352–362. [Google Scholar] [CrossRef]
  33. Yang, S.; Li, L.; Xiao, T.; Zhang, Y.; Zheng, D. Promoting effect of ammonia modification on activated carbon catalyzed peroxymonosulfate oxidation. Sep. Purif. Technol. 2016, 160, 81–88. [Google Scholar] [CrossRef]
  34. Li, Y.; Zhou, W.; Wang, H.; Xie, L.; Liang, Y.; Wei, F.; Idrobo, J.C.; Pennycook, S.J.; Dai, H. An oxygen reduction electrocatalyst based on carbon nanotube-graphene complexes. Nat. Nanotechnol. 2012, 7, 394–400. [Google Scholar] [CrossRef] [PubMed]
  35. Jaouen, F.; Herranz, J.; Lefevre, M.; Dodelet, J.P.; Kramm, U.I.; Herrmann, I.; Bogdanoff, P.; Maruyama, J.; Nagaoka, T.; Garsuch, A.; et al. Cross-laboratory experimental study of non-noble-metal electrocatalysts for the oxygen reduction reaction. ACS Appl. Mater. Interfaces 2009, 1, 1623–1639. [Google Scholar] [CrossRef] [PubMed]
  36. Zhu, Y.; Zhang, B.; Liu, X.; Wang, D.W.; Su, D.S. Unravelling the structure of electrocatalytically active Fe–N complexes in carbon for the oxygen reduction reaction. Angew. Chem. Int. Ed. 2014, 53, 10673–10677. [Google Scholar] [CrossRef] [PubMed]
  37. Cheng, T.; Yu, H.; Peng, F.; Wang, H.; Zhang, B.; Su, D. Identifying active sites of CoNC/CNT from pyrolysis of molecularly defined complexes for oxidative esterification and hydrogenation reactions. Catal. Sci. Technol. 2016, 6, 1007–1015. [Google Scholar] [CrossRef]
  38. Liu, W.; Zhang, L.; Yan, W.; Liu, X.; Yang, X.; Miao, S.; Wang, W.; Wang, A.; Zhang, T. Single-atom dispersed Co–N–C catalyst: Structure identification and performance for hydrogenative coupling of nitroarenes. Chem. Sci. 2016, 7, 5758–5764. [Google Scholar] [CrossRef]
  39. Chen, G.; Zhao, Y.; Fu, G.; Duchesne, P.N.; Gu, L.; Zheng, Y.; Weng, X.; Chen, M.; Zhang, P.; Pao, C.-W.; et al. Interfacial effects in iron-nickel hydroxide-platinum nanoparticles enhance catalytic oxidation. Science 2014, 344, 495–499. [Google Scholar] [CrossRef] [PubMed]
  40. Li, X.; Ao, Z.; Liu, J.; Sun, H.; Rykov, A.I.; Wang, J. Topotactic transformation of metal-organic frameworks to graphene-encapsulated transition-metal nitrides as efficient fenton-like catalysts. ACS Nano 2016, 10, 11532–11540. [Google Scholar] [CrossRef] [PubMed]
  41. Yao, Y.J.; Cai, Y.M.; Lu, F.; Wei, F.Y.; Wang, X.Y.; Wang, S.B. Magnetic recoverable MnFe2O4 and MnFe2O4-graphene hybrid as heterogeneous catalysts of peroxymonosulfate activation for efficient degradation of aqueous organic pollutants. J. Hazard. Mater. 2014, 270, 61–70. [Google Scholar] [CrossRef] [PubMed]
  42. Duan, X.; Ao, Z.; Sun, H.; Indrawirawan, S.; Wang, Y.; Kang, J.; Liang, F.; Zhu, Z.H.; Wang, S. Nitrogen-doped graphene for generation and evolution of reactive radicals by metal-free catalysis. ACS Appl. Mater. Interfaces 2015, 7, 4169–4178. [Google Scholar] [CrossRef] [PubMed]
  43. Wang, Y.; Sun, H.; Duan, X.; Ang, H.M.; Tadé, M.O.; Wang, S. A new magnetic nano zero-valent iron encapsulated in carbon spheres for oxidative degradation of phenol. Appl. Catal. B 2015, 172–173, 73–81. [Google Scholar] [CrossRef]
  44. Sun, H.; Zhou, G.; Liu, S.; Ang, H.M.; Tade, M.O.; Wang, S. Nano-Fe(0) encapsulated in microcarbon spheres: Synthesis, characterization, and environmental applications. ACS Appl. Mater. Interfaces 2012, 4, 6235–6241. [Google Scholar] [CrossRef] [PubMed]
  45. Du, Y.; Ma, W.; Liu, P.; Zou, B.; Ma, J. Magnetic CoFe2O4 nanoparticles supported on titanate nanotubes (CoFe2O4-TNTs) as a novel heterogeneous catalyst for peroxymonosulfate activation and degradation of organic pollutants. J. Hazard. Mater. 2016, 308, 58–66. [Google Scholar] [CrossRef] [PubMed]
  46. Feng, Y.; Wu, D.; Deng, Y.; Zhang, T.; Shih, K. Sulfate radical-mediated degradation of sulfadiazine by CuFeO2 rhombohedral crystal-catalyzed peroxymonosulfate: Synergistic effects and mechanisms. Environ. Sci. Technol. 2016, 50, 3119–3127. [Google Scholar] [CrossRef] [PubMed]
  47. Cai, C.; Zhang, H.; Zhong, X.; Hou, L.W. Electrochemical enhanced heterogeneous activation of peroxydisulfate by Fe-Co/SBA-15 catalyst for the degradation of orange II in water. Water Res. 2014, 66, 473–485. [Google Scholar] [CrossRef] [PubMed]
  48. Deng, J.; Shao, Y.S.; Gao, N.Y.; Tan, C.Q.; Zhou, S.Q.; Hu, X.H. CoFe2O4 magnetic nanoparticles as a highly active heterogeneous catalyst of oxone for the degradation of diclofenac in water. J. Hazard. Mater. 2013, 262, 836–844. [Google Scholar] [CrossRef] [PubMed]
  49. Wang, J.H.; Ozawa, K.; Takahashi, M.; Takeda, M.; Nonami, T. Photocatalytic properties and Sb-121 Mössbauer spectra of antimonic acid fine nanoparticles prepared by soft chemical solution process. Chem. Mater. 2006, 18, 2261–2264. [Google Scholar] [CrossRef]
  50. Ozawa, K.; Wang, H.; Ye, J.; Sakka, Y.; Amano, M. Preparation and some electrical properties of yttrium-doped antimonic acids. Chem. Mater. 2003, 15, 928–934. [Google Scholar] [CrossRef]
  51. Klencsár, Z. MossWinn Manual 2016. Available online: http://www.mosswinn.hu/downloads/mosswinn.pdf (accessed on 26 April 2017).
Figure 1. XRD patterns of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Figure 1. XRD patterns of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Catalysts 07 00138 g001
Figure 2. SEM images of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Figure 2. SEM images of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Catalysts 07 00138 g002
Figure 3. TEM images of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Figure 3. TEM images of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Catalysts 07 00138 g003
Figure 4. N2 adsorption-desorption isotherms (A) and pore size distributions (B) of cobalt-iron catalysts (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Figure 4. N2 adsorption-desorption isotherms (A) and pore size distributions (B) of cobalt-iron catalysts (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Catalysts 07 00138 g004
Figure 5. 57Fe Mössbauer spectra of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Figure 5. 57Fe Mössbauer spectra of cobalt-iron catalysts prepared under different calcination atmospheres and temperatures (a) CFA-500; (b) CFA-600; (c) CFN-500; (d) CFN-600; (e) CFNH-500 and (f) CFNH-600.
Catalysts 07 00138 g005
Figure 6. XPS spectra of CFA-600 in different regions (a) survey; (b) Co 2p; (c) Fe 2p and (d) O 1s.
Figure 6. XPS spectra of CFA-600 in different regions (a) survey; (b) Co 2p; (c) Fe 2p and (d) O 1s.
Catalysts 07 00138 g006
Figure 7. XPS spectra of CFN-600 in different regions (a) survey; (b) Co 2p; (c) Fe 2p and (d) C 1s.
Figure 7. XPS spectra of CFN-600 in different regions (a) survey; (b) Co 2p; (c) Fe 2p and (d) C 1s.
Catalysts 07 00138 g007
Figure 8. XPS spectra of CFNH-600 in different regions (a) survey; (b) Co 2p; (c) Fe 2p; (d) C 1s; (e) N 1s and (f) O 1s.
Figure 8. XPS spectra of CFNH-600 in different regions (a) survey; (b) Co 2p; (c) Fe 2p; (d) C 1s; (e) N 1s and (f) O 1s.
Catalysts 07 00138 g008
Figure 9. The Orange II degradation curves (A) and reaction rate constants k (B) calculated from ln(C0/C) versus time curves of PMS activated Orange II degradation processes observed on different samples (a) no catalysts; (b) CFA-600; (c) CFN-600; and (d) CFNH-600. (Conditions: Orange II, 50 mg L−1; Catalysts, 0.1 g L−1; Oxone, 0.5 g L−1; T = 22 ± 1 °C).
Figure 9. The Orange II degradation curves (A) and reaction rate constants k (B) calculated from ln(C0/C) versus time curves of PMS activated Orange II degradation processes observed on different samples (a) no catalysts; (b) CFA-600; (c) CFN-600; and (d) CFNH-600. (Conditions: Orange II, 50 mg L−1; Catalysts, 0.1 g L−1; Oxone, 0.5 g L−1; T = 22 ± 1 °C).
Catalysts 07 00138 g009
Figure 10. Reusability in Orange II degradation on different samples (a) CFA-600; (b) CFN-600 (14 min); (c) CFNH-600 and (d) CFN-600 (80 min). (Conditions: Orange II, 50 mg L1; Catalysts, 0.1 g L1; Oxone, 0.5 g L1).
Figure 10. Reusability in Orange II degradation on different samples (a) CFA-600; (b) CFN-600 (14 min); (c) CFNH-600 and (d) CFN-600 (80 min). (Conditions: Orange II, 50 mg L1; Catalysts, 0.1 g L1; Oxone, 0.5 g L1).
Catalysts 07 00138 g010
Figure 11. XPS spectra of the used CFA-600 (a) Co 2p3/2; (b) Fe 2p and CFN-600 (c) Co 2p3/2; (d) Fe 2p.
Figure 11. XPS spectra of the used CFA-600 (a) Co 2p3/2; (b) Fe 2p and CFN-600 (c) Co 2p3/2; (d) Fe 2p.
Catalysts 07 00138 g011
Figure 12. High resolution XPS spectra of the used CFNH-600 in different regions (a) S 2p before and after reaction; (b) Co 2p; (c) Fe 2p; (d) C 1s; (e) N 1s and (f) O 1s.
Figure 12. High resolution XPS spectra of the used CFNH-600 in different regions (a) S 2p before and after reaction; (b) Co 2p; (c) Fe 2p; (d) C 1s; (e) N 1s and (f) O 1s.
Catalysts 07 00138 g012
Figure 13. 57Fe Mössbauer spectra of the used CFA-600 (a); CFN-600 (b) and CFNH-600 (c).
Figure 13. 57Fe Mössbauer spectra of the used CFA-600 (a); CFN-600 (b) and CFNH-600 (c).
Catalysts 07 00138 g013
Figure 14. Radical scavenger tests of (a) CFA-600; (b) CFN-600 and (c) CFNH-600.
Figure 14. Radical scavenger tests of (a) CFA-600; (b) CFN-600 and (c) CFNH-600.
Catalysts 07 00138 g014

Share and Cite

MDPI and ACS Style

Zhu, K.; Jin, C.; Klencsár, Z.; Ganeshraja, A.S.; Wang, J. Cobalt-iron Oxide, Alloy and Nitride: Synthesis, Characterization and Application in Catalytic Peroxymonosulfate Activation for Orange II Degradation. Catalysts 2017, 7, 138. https://doi.org/10.3390/catal7050138

AMA Style

Zhu K, Jin C, Klencsár Z, Ganeshraja AS, Wang J. Cobalt-iron Oxide, Alloy and Nitride: Synthesis, Characterization and Application in Catalytic Peroxymonosulfate Activation for Orange II Degradation. Catalysts. 2017; 7(5):138. https://doi.org/10.3390/catal7050138

Chicago/Turabian Style

Zhu, Kaixin, Changzi Jin, Zoltán Klencsár, Ayyakannu Sundaram Ganeshraja, and Junhu Wang. 2017. "Cobalt-iron Oxide, Alloy and Nitride: Synthesis, Characterization and Application in Catalytic Peroxymonosulfate Activation for Orange II Degradation" Catalysts 7, no. 5: 138. https://doi.org/10.3390/catal7050138

APA Style

Zhu, K., Jin, C., Klencsár, Z., Ganeshraja, A. S., & Wang, J. (2017). Cobalt-iron Oxide, Alloy and Nitride: Synthesis, Characterization and Application in Catalytic Peroxymonosulfate Activation for Orange II Degradation. Catalysts, 7(5), 138. https://doi.org/10.3390/catal7050138

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop