Next Article in Journal
Active Brownian Filamentous Polymers under Shear Flow
Next Article in Special Issue
Nanomechanics and Nanorheology of Microgels at Interfaces
Previous Article in Journal
How Green is Your Plasticizer?
Previous Article in Special Issue
Fluid Dynamics of Microgel-Covered Drops Reveal Impact on Interfacial Conditions
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Graphene Oxide Reinforced Alginate/PVA Double Network Hydrogels for Efficient Dye Removal

1
Chemical Engineering and Pharmaceutics School, Henan University of Science and Technology, Luoyang 471023, China
2
Material Science and Engineering School, Zhengzhou University, Zhengzhou 450001, China
*
Authors to whom correspondence should be addressed.
Polymers 2018, 10(8), 835; https://doi.org/10.3390/polym10080835
Submission received: 8 June 2018 / Revised: 24 July 2018 / Accepted: 25 July 2018 / Published: 28 July 2018
(This article belongs to the Special Issue Microgels and Hydrogels at Interfaces)

Abstract

:
Dually crosslinked graphene oxide reinforced alginate/polyvinyl alcohol (PVA) double network (DN) hydrogels were prepared via a facile freeze/thaw method followed by soaking in a Ca2+ solution. The morphology and structure of the hydrogels were systematically examined by Fourier transform infrared spectroscopy (FTIR), X-ray diffraction (XRD), scanning electron microscopy (SEM), and thermogravimetric analysis (TGA). The effects of pH, dosage of hydrogel, adsorption time, and temperature on the adsorptive property of DN hydrogels towards methylene blue (MB) were also studied. Results indicated that the hydrogels exhibited typical 3D porous structures and had an efficient adsorption effect towards MB due to strong interactions between DN hydrogels and MB molecules. The adsorption isotherm was found to coincide with the Langmuir model with a monolayer adsorption. The highest adsorption capacity of DN hydrogels for MB was examined as 480.76 mg·g−1.

Graphical Abstract

1. Introduction

Water pollution originating from all kinds of organic dyes is on the rise due to the rapid development of printing, dyeing, and chemical industry. On account of containing strongly toxic, highly colored, and poorly biodegradable organic dyes, dyestuff wastewater affects the ecological environment and human health seriously [1,2,3]. Methylene blue (MB) is a water-soluble azo dye extensively used for dye printing, biological staining, as a chemical indicator, and so on. In order to reduce the pollution of dyes to water, contamination of MB for instance, many sewage treatment technologies, including biological treatment, chemical oxidation, catalytic ozonation, membrane separation, and adsorption have been developed so far [4,5,6]. Among them, adsorption is a simple, effective, low-cost, and highly available method. However, the exploitation of highly efficient, environmentally friendly adsorbents remains a challenge due to the complexity of wastewater.
In recent years, hydrogels with 3D structures as adsorptive materials for the purpose of dye wastewater treatment have drawn widespread attention [7,8,9]. Dye molecules can permeate into 3D hydrogels with high adsorption rates, integrating with molecular chains of hydrogels by forming hydrogen bonding or electrostatic interactions; therefore, these dye molecules can be readily immobilized by the hydrogel chains. Consequently, porous hydrogels exhibit high adsorption capacities towards different dyes via their versatile structures and properties. Sodium alginate (SA) is a biological linear natural polymer with the merits of biodegradability, low-cost, and non-toxic properties as well as a wealth of sources. It has been widely studied in wastewater treatment applications because of its preferable adsorption property [10,11]. However, the hydrogels obtained from SA exhibit drawbacks such as decreased strength, low superficial area, and weak chemical stability, therefore restricting its application in wastewater treatment. Double network (DN) hydrogels comprising two interpenetrating and cross-linked polymer networks have gained tremendous attention due to their enhanced mechanical property. Many investigations have reported that DN hydrogels exhibited improved mechanical properties and high adsorption capacities for heavy metals and dyes [12,13,14]. For example, a SA/polyvinyl alcohol (PVA) DN hydrogel was prepared for the purpose of achieving enhanced mechanical properties and electrical conductivity [15]. Moreover, the DN hydrogels can be further reinforced by incorporating inorganic materials, such as graphene sheets.
So far, graphene and its derivates have attracted enormous interest due to their unique properties, such as large special surface area, excellent mechanical properties, and unapproachable barrier properties [16,17,18,19]. Compared with hydrophobic graphene, graphene oxide (GO) sheets decorated with a mass of hydroxyl, carboxyl, epoxy, and carboxide groups exhibit good water solubility and benign compatibility with hydrogels [20]. For example, a mechanically robust and printable 3D hydrogel based on alginate and graphene oxide was reported by Liu et al. [21]. However, there have been few studies conducted to examine the influence of graphene sheets on DN hydrogels. Based on these considerations, we herein report a graphene oxide reinforced SA/PVA DN hydrogel for MB adsorption application via a facile freeze/thaw method followed by soaking in a Ca2+ solution. The construction of SA/PVA DN structures greatly increased the mechanical property of SA hydrogels. Meanwhile, the incorporation of graphene oxide sheets into the hydrogels not only further enhanced the mechanical property, but also affected the morphology of the DN hydrogels, yielding smaller pore size and larger pore density.

2. Experimental

2.1. Materials

Sodium alginate (Mw ~250,000 g·mol−1), polyvinyl alcohol (Mw ~74,800 g·mol−1), concentrated sulfuric acid (95%), hydrochloric acid, potassium permanganate, sodium nitrate, and hydrogen peroxide (30%) were purchased from Sinopharm Chemical Reagent Co. Ltd., Shanghai, China. Natural flake graphite (>99%) was bought from Nanjing Pionerr Nano Co. Ltd., Nanjing, China. Anhydrous calcium chloride was purchased from Tianjin Fengchuan Chemical Reagent Technologies Co. Ltd., Tianjin, China. All materials were directly used without further purification.

2.2. Fabrication of Graphene Oxide (GO) Reinforced SA/PVA DN Hydrogels

Graphite oxide was prepared by a modified Hummer’s method [22]. The as-prepared brown graphite oxide was purified by washing with huge amounts of deionized (DI) water to remove residual acids. Then, graphite oxide sponge was obtained by freeze drying. Finally, 0.5 g graphite oxide sponge was ultrasonicated in 500 mL DI water for 30 min to get a brown GO solution.
PVA solution was prepared by dissolving 5 g PVA powder in 100 mL DI water under continuous magnetic stirring at 90 °C. After natural cooling, 5 g SA powder was added into the PVA solution. After magnetic stirring for 2 h, the uniform mixture was degassed and then poured into a mould. Subsequently, the mixture was placed in a freezer and kept at −20 °C for 18 h. Then, the frozen hydrogels were allowed to thaw at room temperature (RT) until the ice melted. This freezing/thawing process was repeated 3 times to form physical crosslinked points between PVA chains. Finally, the hydrogel specimens were dipped into a 4 wt % CaCl2 (200 mL) solution for 6 h to crosslink SA chains, yielding SA/PVA DN hydrogels. Residual Ca2+ within the DN hydrogels was removed by swelling hydrogels in a mass of DI water. GO reinforced SA/PVA DN hydrogels were prepared by the same procedures with loadings of 100, 300, 500, and 700 mg GO, respectively. The as-prepared hydrogels with GO contents of 1, 3, 5, and 7 wt % were designated as GO1-SA/PVA, GO3-SA/PVA, GO5-SA/PVA, and GO7-SA/PVA, respectively. The preparation procedures and crosslinking mechanisms of the GO reinforced DN hydrogels are schematically represented in Figure 1.

2.3. Characterizations

Fourier transform infrared (FTIR) measurement was carried out by using a potassium bromide micropellet technique on a Nicolet iS50 spectrometer (Thermo Fisher Scientific, Waltham, MA, USA). X-ray diffraction (XRD) analysis was performed on a D8 X-ray diffractometer (40 kV, 40 mA, λ = 0.154 nm, Bruker, Karlsruhe, Germany) by using a powder diffraction method. Thermogravimetric analysis was conducted by a TQ50 from room temperature to 700 °C at a heating rate of 10 °C·min−1 in nitrogen flow (TA Instruments, New Castle, DE, USA). Prior to scanning electron microscopy (SEM) study, the fractured freeze-dried hydrogels were coated with a thin layer of gold (JSM-5610LV, Japan Electronics Co. Ltd., Tokyo, Japan). The detection of MB concentration was performed using a UV–visible spectrophotometer (UV5200, Metash instrument Co. Ltd., Shanghai, China). Tensile test experiments were carried out on a CMT6104 electronic-universal testing machine (Shenzhen Skyan Power Equipment Co. Ltd., Shenzhen, China).

2.4. MB Adsorption Studies

MB adsorption experiment was performed by shaking a certain mass of GO reinforced DN hydrogels in 25 mL MB solution with an agitating speed of 100 rpm at 30 °C for 15 h to reach the absorbance equilibrium state. HCl and NaOH solutions were used in order to adjust the pH values of the adsorption solutions. Absorbance of the solution was measured by a UV–visible spectrophotometer under a wavelength of 664 nm. The influences of GO loadings (under pH 6.5) and pH on the adsorption were examined by soaking a 0.025 g sample into 25 mL of MB solution (200 mg·L−1) for 15 h. The influence of the initial concentration of MB on the adsorption was performed by adding 0.025 g of specimen into 25 mL of MB solution (50, 100, 150, 200, 300, 400, 500, 700, and 900 mg·L−1, respectively) for 15 h (pH = 6.5). The effect of contact time on the adsorption was investigated by soaking 0.15 g of sample into 150 mL of MB solution under pH of 6.5. The adsorption capacity (qt) and removal efficiency (Re) were calculated from the following expressions:
q t = ( C 0 C t ) V m
R e ( % ) = C 0 C t C 0 × 100 %
where qt is the adsorption capacity (mg·g−1) and C0 is the initial MB concentration, whereas Ct is the MB concentration at any time, t (mg·L−1). V was the volume of the experimental solution (mL) and m was the mass of adsorbent (g).
In order to investigate the adsorption process and adsorption mechanism of GO reinforced DN hydrogels, three kinds of adsorption kinetic equations, namely, the pseudo-first-order equation, pseudo-second-order equation, and intraparticle diffusion equation, were used to fit the experimental data [23].
The pseudo-first-order kinetic model is expressed as:
ln ( q e q t ) = ln q e k 1 t
where qt and qe stand for the adsorption capacities of DN hydrogels (mg·g−1) at t and the equilibrium state, respectively. k1 (min−1) is the rate constant.
The pseudo-second-order equation is expressed as:
t q t = 1 k 2 q e 2 + t q e
where k2 (g·mg−1·min−1) is the pseudo-second-order adsorption rate constant.
The intraparticle diffusion model is expressed as:
q t = k i t 1 2 + C
where ki is the rate constant of the intraparticle diffusion model (mg∙g−1·min−1/2) and C is a constant standing for the boundary layer effects.

3. Results and Discussion

3.1. Formation Mechanism of GO Reinforced SA/PVA DN Hydrogels

The dual crosslinking mechanisms of GO reinforced SA/PVA DN hydrogels were schematically presented in Figure 1. As could be seen, PVA chains were crosslinked by forming crystalline regions during the freezing/thawing treatments of PVA solution. On the other hand, alginate chains were crosslinked by Ca2+ ions, as described elsewhere [24]. Furthermore, the presence of GO offered hydrogen bonding interaction between GO sheets and PVA/SA chains. Therefore, GO sheets worked as additional crosslinking points in SA/PVA DN hydrogels. This conclusion was further confirmed by FTIR and SEM studies.

3.2. FTIR Analysis

FTIR spectrometry was employed for monitoring the interactions between GO sheets and polymer networks. As shown in Figure 2, the FTIR spectrum of GO exhibited characteristic peaks of –OH, C=O, C=C, and C–O–C at 3420, 1731, 1633, and 1237 cm−1, respectively. For neat SA/PVA, the predominant peaks located at 3348 and 2922 are ascribed to the stretching vibrations of –OH and –CH2, respectively. The peaks at 1608 and 1438 cm−1 are attributed to the asymmetric and symmetric stretching vibrations of carboxylate ions, respectively [25]. The characteristic peak located at 1093 cm−1 was due to the stretching vibration of C–O–C. In comparison with neat SA/PVA, GO reinforced SA/PVA DN hydrogels exhibited lower wave numbers, possibly due to the dissociation of hydrogen bonding among the hydroxyl groups in PVA and formation of new hydrogen bonding between the hydroxyl groups of PVA/SA with hydroxyl groups of GO sheets [18].

3.3. Thermogravimetric Analysis

TGA (TA Instruments, New Castle, DE, USA) and corresponding differential thermogravimetric analysis (DTG) curves are shown in Figure 3a,b, respectively. TGA thermograms exhibited the good thermal stability of specimens below 250 °C. This slight weight loss (8%) was attributed to the dissociation of water [19]. Sharp mass loss was observed around 265–340 °C due to the decomposition of polymer networks. It was noted that the weight loss of DN hydrogels with different GO loadings differed greatly. GO3-SA/PVA exhibited a weight loss of 52%, whereas GO1-SA/PVA exhibited a weight loss of 48%. However, the introduction of GO into SA/PVA DN hydrogels did not improve its thermal stability much.

3.4. XRD Analysis

Figure 4 shows the XRD patterns of GO and GO reinforced SA/PVA specimens. As was shown, the XRD pattern of GO exhibited a sharp peak at 2θ = 19.5°. In the case of neat SA/PVA, the peak located at 2θ = 11.9° was due to the amorphous diffraction peak of SA. The peaks located at 2θ = 32°, 34°, and 45° were due to the presence of excrescent calcium ions in SA [26]. The sharp peak presented at 2θ = 20.2° was ascribed to the diffraction peak of PVA [18]. Interestingly, with increasing contents of GO, the intensity of the PVA peak increased slightly, followed by decreasing greatly. The changes in peak intensity demonstrated the corresponding changes in the degree of crystallinity of the SA/PVA hydrogels. It had been reported that the introduction of GO could affect the degree of crystallinity of PVA [18]. The largest degree of crystallinity of PVA in GO1-SA/PVA indicated that the PVA chains in GO1-SA/PVA exhibited the biggest physical crosslinking density by forming crystalline regions. Therefore, it was reasonable to observe the variation tendency in the XRD diffraction peaks of GO reinforced DN SA/PVA hydrogels. The reason was that the addition of nanofiller GO could impact on the crystallization behavior of crystalline polymers due to the heterogeneous nucleation of GO sheets. On the other hand, GO1-SA/PVA also exhibited the highest peaks at 2θ = 32° and 34°, in comparison to other diffraction peaks. This might be due to the relatively higher amount of residual calcium ions inside the GO1-SA/PVA.

3.5. SEM Characterization

For further investigating the influence of GO sheets on the morphology of SA/PVA DN hydrogels, samples with different GO loadings were freeze-dried, then coated with a thin layer of gold and subjected to SEM examinations. The results were shown in Figure 5. It could be observed that all SA/PVA DN hydrogels exhibited a porous 3D structure, consistent with previous reports [27,28]. However, with increasing GO contents, the SA/PVA composites exhibited smaller pore size, demonstrating the formation of an improved degree of crosslinking. The crosslinking of SA/PVA by GO sheets via hydrogen bonding interactions accounted for this improved degree of crosslinking. Moreover, this increased degree of crosslinking could also enhance the mechanical property of SA/PVA DN hydrogels.

3.6. Mechanical Properties

The stress-strain curves of the SA/PVA DN hydrogels with different GO loadings are shown in Figure 6. It is known that the degree of crystallinity, degree of crosslinking, and nanofiller dosage can influence the mechanical properties of composites greatly. As depicted, with increasing GO amounts, the SA/PVA DN hydrogels exhibited a tendency to decrease after an increase in degree of crystallinity. On the other hand, the degree of crosslinking was always increased with increasing GO contents. On account of the enhancements by GO sheets and degree of crosslinking, the fracture strength of GO reinforced SA/PVA hydrogels increased from 0.11 MPa for neat SA/PVA to 0.24 MPa for GO7-SA/PVA. In addition, it is worthy to note that the elongation at break of the composite hydrogels increased first, followed by decreasing. The increase in elongation at break for SA/PVA DN hydrogels with a small amount of GO can be ascribed to the formation of hydrogen bonding interaction between GO and polymer chains, as described by Fan et al. [29]. However, excessive embedment of GO sheets will restrict the elasticity of the polymer chains, therefore resulting in a reduction in elongation at break [30].

3.7. MB Adsorption

As described previously in Figure 5, GO content affects the morphology of the GO reinforced DN hydrogels greatly. With loading more GO, the composite hydrogels exhibit smaller pore size and higher porosity, therefore affecting the adsorption behavior of MB. The influence of GO content on the adsorption of DN hydrogels for MB is shown in Figure 7a. It can be observed that increased GO content results in an improved adsorption capacity for MB. First, higher GO content results in higher porosity and larger specific area, which can obviously improve the adsorption capacity. Second, GO sheets were functionalized with a vast number of hydroxyl and carboxyl groups. These versatile groups can interact with MB molecules by electrostatic or hydrogen bonding interactions. Finally, GO and MB molecules can have strong π–π interactions. Based on these factors, improving GO content produces enhanced adsorption capacity. However, when the GO content is higher than 5%, the increase tendency in adsorption capacity is slowed down, probably due to the aggregation of GO sheets.
pH is one of the important factors which influence the adsorption properties of DN hydrogel for MB. The effect of pH on the MB adsorption is shown in Figure 7b. As can be seen, with increasing the pH values of the solution from 2.4 to 6.4, the adsorption capacity increases greatly from 123.40 to 165.51 mg·g−1. On the other hand, when further increasing the pH values from 6.4 to 9.5, the adsorption capacity does not change much. Due to the presence of versatile oxygen-containing groups decorated in DN hydrogels, such as hydroxyl and carboxyl groups, MB can be adsorbed onto the DN hydrogels by either electrostatic interaction or hydrogen bonding interaction. Different pH values not only influence the charge distribution of DN hydrogels, but also the ionization of DN hydrogels and MB. Therefore, the adsorption behavior of DN hydrogels towards MB was greatly influenced by pH values. At low pH values, the carboxyl groups of SA and GO were protonated. Consequently, it reduces the electrostatic interactions between the DN hydrogels and MB molecules. In addition, excess proton ions will transform the hydroxyl groups of DN hydrogels into –OH2+ groups. Then, the electrostatic repulsion between –OH2+ groups and cationic dye MB further reduces the adsorption capacity [31,32]. Hence, at low pH values, the DN hydrogels exhibit extremely low adsorption capacities. When increasing pH values, the carboxyl groups of DN hydrogels were unprotonated as anions; the electrostatic interaction between the carboxylate radical and MB molecules accounts for the increased adsorption capacities for MB. The optimum pH was determined to be 6.4 for MB [33].
The effect of DN hydrogel dosage on the adsorption was examined by soaking different amounts of hydrogels into 25 mL of MB solution with a concentration of 200 mg·L−1. As can be seen from Figure 8a, the equilibrium adsorption capacity of DN hydrogels for MB was decreased with increasing the dosage of DN hydrogels. When the dosages of DN hydrogel were changed from 0.5 to 8 g·L−1, the equilibrium adsorption capacities were reduced from 313.09 to 23.09 mg·g−1. For a certain amount of MB solution, DN hydrogels with lowered dosages would readily reach a saturation adsorption state due to the limited adsorption active points in DN hydrogels [34]. However, when increasing the dosage of DN hydrogels, the adsorption active points were in an unsaturated adsorption state, resulting in lowered adsorption capacities. The optimum adsorbent dosage was determined to be 1.00 g·L−1 for MB.
The influence of contact time on the adsorption was shown in Figure 8b. As can be seen, DN hydrogels exhibit similar adsorption behavior for MB solutions with different concentrations. At the beginning of the adsorption, the adsorption capacity increases with increasing the contact time. This might be due to the large content of MB at the initial state, resulting in convenience for the MB to diffuse into the DN hydrogels. Upon further increasing contact time, the number of MB molecules in solution reduced and the active adsorption points in DN hydrogels were occupied by MB molecules, therefore resulting in a moderate increase in adsorption capacity [35].
The corresponding kinetic parameters and determination coefficients obtained from the slope and intercept according to these equations are shown in Table 1 and Table 2.
In comparison with the pseudo-first-order model, the theoretical equilibrium adsorption capacities of the pseudo-second-order model shown in Figure 9b and Table 1 are closer to the experimental values. In addition, the correlation coefficients (R2) of the pseudo-second-order model are larger than that of the pseudo-first-order model, indicating that the pseudo-second-order model was applicable to the MB adsorption process [32]. Furthermore, the theoretical adsorption capacities of MB increase with increasing MB concentration, whereas the adsorption rate constant of the pseudo-second-order model decreases with increasing MB concentration due to the hindrance of higher concentrations of MB. After disclosing the adsorption process, the adsorption mechanism was further discussed by using the intraparticle diffusion model.
According to Figure 9c, all plots don’t pass through the origin, indicating that intraparticle diffusion was not the sole rate-controlling step. However, the majority of the correlation coefficients in Table 2 were larger than 0.98, demonstrating the adsorption mechanism can be explained by the intra-particle diffusion model. There are two stages in the adsorption curves of MB by DN hydrogels exhibiting different slopes. In the first stage, MB molecules diffuse from the solution into the surface of the DN hydrogels through large pores or channels inside the porous DN hydrogels. In the second stage, MB molecules diffuse into smaller pores and finally reach the equilibrium state [36].
Langmuir and Freundlich adsorption isothermal equations are widely used to describe the chemical adsorption behaviours [37]. Langmuir adsorption isotherm relies on the monolayer adsorption and the adsorption points being distributed uniformly among the surface of the adsorbent. The interaction between adsorbent and adsorbate is assumed to be strong enough. The Langmuir adsorption isotherm is expressed as:
C e q e = 1 q m K L + C e q m
where qe and ce are the equilibrium adsorption capacity (mg·g−1) and equilibrium concentration (mg·g−1), respectively. qm is the maximum adsorption capacity (mg·g−1) and KL is the rate constant of Langmuir adsorption isotherm.
Freundlich adsorption isothermal is an empirical equation; normally used for elucidating a nonideal adsorption behaviour of adsorbent, it can be expressed as:
log q e = log K F + 1 n log C e
where KF is the rate constant of the Freundlich adsorption isotherm. 1/n is a constant related to adsorption capacity. According to Table 3, the 1/n value is 0.44, indicating that MB is easily adsorbed onto DN hydrogels by a Freundlich adsorption model.
The experimental data were fitted with the Langmuir and Freundlich adsorption isothermal equations, respectively, and the results are shown in Figure 10 and Table 3. The correlation coefficient (R2) of the Langmuir adsorption model is 0.9896, larger than that of the Freundlich adsorption model (0.9635), demonstrating that the Langmuir adsorption model is more in accord with the experimental data in comparison with the Freundlich adsorption model.
In order to investigate the influence of temperature on the adsorption process, an adsorption experiment was performed at 298, 303, 313, and 323 K, respectively. Thermodynamic parameters, such as ΔG, ΔH, and ΔS were determined as:
K c = q e C e
ln K c = Δ S R Δ H R T
Δ G = Δ H T Δ S
where T (K) is temperature and ΔH (kJ∙mol−1), ΔS (J mol−1 K−1), and ΔG (kJ∙mol−1) are the changes in enthalpy, entropy, and Gibbs free energy, respectively.
The results are given in Table 4. As is shown, all ΔG values are negative, indicating that the adsorption of MB is a spontaneous process. Furthermore, the value of ΔG increases with improving temperature, demonstrating that low temperature is favourable for MB adsorption. ΔH is negative, demonstrating that the adsorption is an exothermic process. Due to the adsorption of MB molecules onto the surface of DN hydrogels reducing the disorder, the values of ΔS also are negative. This is in line with a previous report [38].

4. Conclusions

In summary, dually crosslinked SA/PVA DN hydrogels reinforced by GO sheets were successfully prepared via a facile freeze/thaw process followed by soaking in a Ca2+ solution. The as-resulted hydrogels exhibited typical 3D porous structures. Contributed by the fascinating GO sheets, the porous hydrogels exhibited enhanced mechanical properties and excellent adsorption behaviors towards MB. Therefore, the GO reinforced SA/PVA DN hydrogels can be used as a nontoxic, biodegradable, low-cost dye adsorbent to treat dyestuff wastewater. The experimental adsorptive data coincided with the Langmuir model. The pseudo-second-order model could describe the adsorption behaviour of the DN hydrogel for MB well. Thermodynamic investigations elucidated that the adsorption of MB by DN hydrogels was a spontaneous and exothermic process.

Author Contributions

C.L. and H.L. designed the experiments and wrote the paper. T.X. prepared the samples. A.X. and B.P. analyzed the data. K.T. contributed to the reagents/materials.

Funding

We gratefully acknowledge the financial supports by research project of HAUST (No. 13480051), National Natural Science Foundation of China (51675162, 21373078, U1704144), Science and Technology Innovation Team Training and Development Plan of HAUST (2015XTD008), Henan Province Science and Technology Research Plan (152102210274).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Shahabuddin, S.; Sarih, N.M.; Kamboh, M.A.; Nodeh, H.R.; Mohamad, S. Synthesis of Polyaniline-Coated Graphene Oxide@SrTiO3 Nanocube Nanocomposites for Enhanced Removal of Carcinogenic Dyes from Aqueous Solution. Polymers 2016, 8, 305. [Google Scholar] [CrossRef]
  2. Elkady, M.; El-Aassar, M.; Hassan, H. Adsorption Profile of Basic Dye onto Novel Fabricated Carboxylated Functionalized Co-Polymer Nanofibers. Polymers 2016, 8, 177. [Google Scholar] [CrossRef]
  3. Liu, C.; Liu, H.; Xu, A.; Tang, K.; Huang, Y.; Lu, C. In situ reduced and assembled three-dimensional graphene aerogel for efficient dye removal. J. Alloys Compd. 2017, 714, 522–529. [Google Scholar] [CrossRef]
  4. Pawar, R.R.; Gupta, P.; Sawant, S.Y.; Shahmoradi, B.; Lee, S.M. Porous synthetic hectorite clay-alginate composite beads for effective adsorption of methylene blue dye from aqueous solution. Int. J. Biol. Macromol. 2018, 114, 1315. [Google Scholar] [CrossRef] [PubMed]
  5. Qian, L.W.; Yang, M.X.; Zhang, S.F.; Hou, C.; Song, W.Q.; Yang, J.F.; Tang, R.H. Preparation of a sustainable bioadsorbent by modifying filter paper with sodium alginate, with enhanced mechanical properties and good adsorption of methylene blue from wastewaters. Cellulose 2018, 25, 2021–2036. [Google Scholar] [CrossRef]
  6. Ai, L.; Li, M.; Li, L. Adsorption of Methylene Blue from Aqueous Solution with Activated Carbon/Cobalt Ferrite/Alginate Composite Beads: Kinetics, Isotherms, and Thermodynamics. J. Chem. Eng. Data 2011, 56, 3475–3483. [Google Scholar] [CrossRef]
  7. Zhu, H.Y.; Fu, Y.Q.; Jiang, R.; Yao, J.; Xiao, L.; Zeng, G.M. Novel magnetic chitosan/poly(vinyl alcohol) hydrogel beads: Preparation, characterization and application for adsorption of dye from aqueous solution. Bioresour. Technol. 2012, 105, 24–30. [Google Scholar] [CrossRef] [PubMed]
  8. Abou, M.T.; Abd, E.M.; Abd, E.R. Radiation preparation of PVA/CMC copolymers and their application in removal of dyes. J. Hazard. Mater. 2009, 168, 68–75. [Google Scholar]
  9. Gong, G.; Zhang, F.; Cheng, Z.; Zhou, L. Facile fabrication of magnetic carboxymethyl starch/poly(vinyl alcohol) composite gel for methylene blue removal. Int. J. Biol. Macromol. 2015, 81, 205–211. [Google Scholar] [CrossRef] [PubMed]
  10. Shao, Z.J.; Huang, X.L.; Yang, F.; Zhao, W.F.; Zhou, X.Z.; Zhao, C.S. Engineering sodium alginate-based cross-linked beads with high removal ability of toxic metal ions and cationic dyes. Carbohydr. Polym. 2018, 187, 85. [Google Scholar] [CrossRef] [PubMed]
  11. Soliman, S.M.A.; Ali, A.M.; Sabaa, M.W. Alginate-based hydrogel for water treatment. Desalination Water Treat. 2017, 94, 129–136. [Google Scholar] [CrossRef]
  12. Zhou, G.; Liu, C.; Chu, L.; Tang, Y.; Luo, S. Rapid and efficient treatment of wastewater with high-concentration heavy metals using a new type of hydrogel-based adsorption process. Bioresour. Technol. 2016, 219, 451–457. [Google Scholar] [CrossRef] [PubMed]
  13. Pourjavadi, A.; Tavakoli, E.; Motamedi, A.; Salimi, H. Facile synthesis of extremely biocompatible double-network hydrogels based on chitosan and poly(vinyl alcohol) with enhanced mechanical properties. J. Appl. Polym. Sci. 2017, 135, 45752. [Google Scholar] [CrossRef]
  14. Ma, J.; Liu, Y.; Ali, O.; Wei, Y.; Zhang, S.; Zhang, Y.; Cai, T.; Liu, C.; Luo, S. Fast Adsorption of Heavy Metal Ions by Waste Cotton Fabrics Based Double Network Hydrogel and Influencing Factors Insight. J. Hazard. Mater. 2017, 344, 1034–1042. [Google Scholar] [CrossRef]
  15. Jiang, X.; Xiang, N.; Zhang, H.; Sun, Y.; Zhen, L.; Hou, L. Preparation and characterization of poly(vinyl alcohol)/sodium alginate hydrogel with high toughness and electric conductivity. Carbohydr. Polym. 2018, 186, 377. [Google Scholar] [CrossRef] [PubMed]
  16. Liu, H.; Liu, C.; Peng, S.; Pan, B.; Lu, C. Effect of polyethyleneimine modified graphene on the mechanical and water vapor barrier properties of methyl cellulose composite films. Carbohydr. Polym. 2018, 182, 52–60. [Google Scholar] [CrossRef] [PubMed]
  17. Liu, H.; Bandyopadhyay, P.; Kshetri, T.; Kim, N.H.; Ku, B.C.; Moon, B.; Lee, J.H. Layer-by-layer assembled polyelectrolyte-decorated graphene multilayer film for hydrogen gas barrier application. Compos. Part B 2017, 114, 339–347. [Google Scholar] [CrossRef]
  18. Liu, H.; Bandyopadhyay, P.; Kim, N.H.; Moon, B.; Lee, J.H. Surface modified graphene oxide/poly(vinyl alcohol) composite for enhanced hydrogen gas barrier film. Polym. Test. 2016, 50, 49–56. [Google Scholar] [CrossRef]
  19. Liu, H.; Kuila, T.; Kim, N.; Ku, B.C.; Lee, J. In situ synthesis of the reduced graphene oxide-polyethyleneimine composite and its gas barrier properties. J. Mater. Chem. A 2013, 1, 3739–3746. [Google Scholar] [CrossRef]
  20. Yu, Y.; Shu, Y.; Ye, L. In Situ Crosslinking of Poly(vinyl alcohol)/Graphene Oxide-Glutamic Acid Nano-composite Hydrogel as Microbial Carrier: Intercalation Structure and its Wastewater Treatment Performance. Chem. Eng. J. 2018, 336, 306–314. [Google Scholar] [CrossRef]
  21. Liu, S.; Bastola, A.K.; Li, L. A 3D Printable and Mechanically Robust Hydrogel based on Alginate and Graphene Oxide. Acs Appl. Mater. Interfaces 2017, 9, 41473–41481. [Google Scholar] [CrossRef] [PubMed]
  22. Qi, Y.; Yang, M.; Xu, W.; He, S.; Men, Y. Natural polysaccharides-modified graphene oxide for adsorption of organic dyes from aqueous solutions. J. Colloid Interface Sci. 2017, 486, 84–96. [Google Scholar] [CrossRef] [PubMed]
  23. Chen, L.; Li, Y.; Du, Q.; Wang, Z.; Xia, Y.; Yedinak, E.; Lou, J.; Ci, L. High performance agar/graphene oxide composite aerogel for methylene blue removal. Carbohydr. Polym. 2017, 155, 345–353. [Google Scholar] [CrossRef] [PubMed]
  24. Kumar, M.; Tamilarasan, R. Modeling studies: Adsorption of aniline blue by using Prosopis Juliflora carbon/Ca/alginate polymer composite beads. Carbohydr. Polym. 2013, 92, 2171–2180. [Google Scholar] [CrossRef] [PubMed]
  25. Xie, M.; Zhang, F.; Liu, L.; Zhang, Y.; Li, Y.; Li, H.; Xie, J. Surface modification of graphene oxide nanosheets by protamine sulfate/sodium alginate for anti-cancer drug delivery application. Appl. Surf. Sci. 2018, 440, 853–860. [Google Scholar] [CrossRef]
  26. Khalid, I.; Ahmad, M.; Minhas, M.U.; Barkat, K. Preparation and characterization of alginate-PVA-based semi-IPN: Controlled release pH-responsive composites. Polym. Bull. 2018, 75, 1075–1099. [Google Scholar] [CrossRef]
  27. Xiang, S.; Qian, W.; Li, T.; Wang, Y.; Chen, M.; Ma, P.; Dong, W. Hierarchical Structural Double Network Hydrogel with High Strength, Toughness, and Good Recoverability. New J. Chem. 2017, 41, 14397–14402. [Google Scholar] [CrossRef]
  28. Wang, Z.; Zhou, H.; Chen, W.; Li, Q.; Yan, B.; Jin, X.; Ma, A.; Liu, H.; Zhao, W. Dually synergetic network hydrogels with integrated mechanical stretchability, thermal responsiveness and electrical conductivity for strain sensors and temperature alertors. Acs Appl. Mater. Interfaces 2018, 10, 14045–14054. [Google Scholar] [CrossRef] [PubMed]
  29. Fan, J.; Shi, Z.; Lian, M.; Li, H.; Yin, J. Mechanically strong graphene oxide/sodium alginate/polyacrylamide nanocomposite hydrogel with improved dye adsorption capacity. J. Mater. Chem. A 2013, 1, 7433–7443. [Google Scholar] [CrossRef]
  30. Liu, C.; Liu, H.; Lu, C.; Tang, K.; Zhang, Y. Polyethyleneimine-modified graphene oxide/PNIPAm thermoresponsive hydrogels with rapid swelling/deswelling and improved mechanical properties. J. Mater. Sci. 2017, 52, 11715–11724. [Google Scholar] [CrossRef]
  31. Cui, L.; Wang, Y.; Hu, L.; Gao, L.; Du, B.; Wei, Q. Mechanism of Pb(II) and methylene blue adsorption onto magnetic carbonate hydroxyapatite/graphene oxide. Rsc Adv. 2015, 5, 9759–9770. [Google Scholar] [CrossRef]
  32. Dai, H.; Huang, Y.; Huang, H. Eco-friendly polyvinyl alcohol/carboxymethyl cellulose hydrogels reinforced with graphene oxide and bentonite for enhanced adsorption of methylene blue. Carbohydr. Polym. 2017, 185, 1–11. [Google Scholar] [CrossRef] [PubMed]
  33. Liu, C.; Omer, A.M.; Ouyang, X.K. Adsorptive removal of cationic methylene blue dye using carboxymethyl cellulose/k-carrageenan/activated montmorillonite composite beads: Isotherm and kinetic studies. Int. J. Biol. Macromol. 2017, 106, 823–833. [Google Scholar] [CrossRef] [PubMed]
  34. Ghorai, S.; Sarkar, A.; Raoufi, M.; Panda, A.B.; Schönherr, H.; Pal, S. Enhanced removal of methylene blue and methyl violet dyes from aqueous solution using a nanocomposite of hydrolyzed polyacrylamide grafted xanthan gum and incorporated nanosilica. Acs Appl. Mater. Interfaces 2014, 6, 4766. [Google Scholar] [CrossRef] [PubMed]
  35. Yang, X.; Li, Y.; Du, Q.; Sun, J.; Chen, L.; Hu, S.; Wang, Z.; Xia, Y.; Xia, L. Highly effective removal of basic fuchsin from aqueous solutions by anionic polyacrylamide/graphene oxide aerogels. J. Colloid Interface Sci. 2015, 453, 107–114. [Google Scholar] [CrossRef] [PubMed]
  36. Chong, C.; Jie, D.; Bei, L.; Ai, H.; Xiang, Z.; Lang, M.; Shuang, L.; Zhao, C. Toward 3D graphene oxide gels based adsorbents for high-efficient water treatment via the promotion of biopolymers. J. Hazard. Mater. 2013, 263, 467–478. [Google Scholar] [CrossRef] [PubMed]
  37. Wang, Y.; Feng, Y.; Zhang, X.F.; Zhang, X.; Jiang, J.; Yao, J. Alginate-based attapulgite foams as efficient and recyclable adsorbents for the removal of heavy metals. J. Colloid Interface Sci. 2017, 514, 190. [Google Scholar] [CrossRef] [PubMed]
  38. Melo, B.C.; Faa, P.; Cardoso, V.A.; Agb, P.; Fajardo, A.R.; Fha, R. Cellulose nanowhiskers improve the methylene blue adsorption capacity of chitosan-g-poly(acrylic acid) hydrogel. Carbohydr. Polym. 2018, 181, 358–367. [Google Scholar] [CrossRef] [PubMed]
Figure 1. Schematic of crosslinking mechanism of graphene oxide (GO) reinforced double network (DN) hydrogel.
Figure 1. Schematic of crosslinking mechanism of graphene oxide (GO) reinforced double network (DN) hydrogel.
Polymers 10 00835 g001
Figure 2. FTIR spectra of GO, DN hydrogel, and DN hydrogels with different GO loadings.
Figure 2. FTIR spectra of GO, DN hydrogel, and DN hydrogels with different GO loadings.
Polymers 10 00835 g002
Figure 3. (a) TGA and (b) differential thermogravimetric analysis (DTG) curves of DN hydrogel and GO reinforced DN hydrogels composites.
Figure 3. (a) TGA and (b) differential thermogravimetric analysis (DTG) curves of DN hydrogel and GO reinforced DN hydrogels composites.
Polymers 10 00835 g003
Figure 4. XRD patterns of GO, neat DN hydrogel, and GO reinforced DN hydrogels.
Figure 4. XRD patterns of GO, neat DN hydrogel, and GO reinforced DN hydrogels.
Polymers 10 00835 g004
Figure 5. SEM images of SA/PVA with different GO loadings: (a) neat SA/PVA; (b) GO1-SA/PVA; (c) GO3-SA/PVA; (d) GO5-SA/PVA; (e) GO7-SA/PVA.
Figure 5. SEM images of SA/PVA with different GO loadings: (a) neat SA/PVA; (b) GO1-SA/PVA; (c) GO3-SA/PVA; (d) GO5-SA/PVA; (e) GO7-SA/PVA.
Polymers 10 00835 g005
Figure 6. Stress-strain curves of neat DN hydrogel and GO reinforced DN hydrogels.
Figure 6. Stress-strain curves of neat DN hydrogel and GO reinforced DN hydrogels.
Polymers 10 00835 g006
Figure 7. Effects of (a) GO content and (b) solution pH on the methylene blue (MB) adsorption.
Figure 7. Effects of (a) GO content and (b) solution pH on the methylene blue (MB) adsorption.
Polymers 10 00835 g007
Figure 8. Effects of (a) dosage of adsorbent and (b) contact time on the MB adsorption.
Figure 8. Effects of (a) dosage of adsorbent and (b) contact time on the MB adsorption.
Polymers 10 00835 g008
Figure 9. (a) Pseudo-first-order plots, (b) pseudo-second-order plots, and (c) intraparticle diffusion plots for MB adsorption.
Figure 9. (a) Pseudo-first-order plots, (b) pseudo-second-order plots, and (c) intraparticle diffusion plots for MB adsorption.
Polymers 10 00835 g009
Figure 10. Langmuir (a) and Freundlich (b) adsorption isotherm models of MB.
Figure 10. Langmuir (a) and Freundlich (b) adsorption isotherm models of MB.
Polymers 10 00835 g010
Table 1. Adsorption kinetic parameters of MB by adsorbents.
Table 1. Adsorption kinetic parameters of MB by adsorbents.
C0 (mg∙L−1)Pseudo-first-order modelPseudo-second-order model
qe (exp)(mg∙g−1)k1 (min−1)qe (cal)(mg∙g−1)R2k2 (g∙mg−1∙min−1)qe (cal)(mg∙g−1)R2
10092.010.003759.770.99121.14 × 10−497.660.9985
200170.120.0029102.780.98995.72 × 10−5179.860.9981
300245.750.0031150.610.98453.93 × 10−5260.420.9977
400295.150.0034181.750.99363.67 × 10−5311.530.9982
Table 2. Parameters of intra-particle diffusion model for MB adsorption.
Table 2. Parameters of intra-particle diffusion model for MB adsorption.
C0 (mg·L−1)Step IStep II
Ki1 (mg·g−1·min−1/2)C (mg·g−1)R2Ki2 (mg·g−1·min−1/2)C (mg·g−1)R2
1003.4913.060.98990.3977.040.9819
2005.9728.210.98681.09127.980.9825
3009.3132.320.99241.61183.070.9929
4009.7060.100.98671.61233.050.9773
Table 3. Adsorption isotherm parameters of Langmuir and Freundlich models.
Table 3. Adsorption isotherm parameters of Langmuir and Freundlich models.
Langmuir modelFreundlich model
qm (mg·g−1)KL (L·mg−1)R2KF1/nR2
480.760.020.989634.110.440.9635
Table 4. Thermodynamic parameters for MB adsorption at different temperatures.
Table 4. Thermodynamic parameters for MB adsorption at different temperatures.
T (K)Kc (L∙mg−1)ΔG (kJ∙mol1)ΔH (kJ∙mol1)ΔS (J∙mol1∙K1)
2986.94−4.80−15.45−35.95
3035.96−4.49
3134.90−4.14
3234.25−3.89

Share and Cite

MDPI and ACS Style

Liu, C.; Liu, H.; Xiong, T.; Xu, A.; Pan, B.; Tang, K. Graphene Oxide Reinforced Alginate/PVA Double Network Hydrogels for Efficient Dye Removal. Polymers 2018, 10, 835. https://doi.org/10.3390/polym10080835

AMA Style

Liu C, Liu H, Xiong T, Xu A, Pan B, Tang K. Graphene Oxide Reinforced Alginate/PVA Double Network Hydrogels for Efficient Dye Removal. Polymers. 2018; 10(8):835. https://doi.org/10.3390/polym10080835

Chicago/Turabian Style

Liu, Cuiyun, Hongyu Liu, Tianhui Xiong, Airong Xu, Bingli Pan, and Keyong Tang. 2018. "Graphene Oxide Reinforced Alginate/PVA Double Network Hydrogels for Efficient Dye Removal" Polymers 10, no. 8: 835. https://doi.org/10.3390/polym10080835

APA Style

Liu, C., Liu, H., Xiong, T., Xu, A., Pan, B., & Tang, K. (2018). Graphene Oxide Reinforced Alginate/PVA Double Network Hydrogels for Efficient Dye Removal. Polymers, 10(8), 835. https://doi.org/10.3390/polym10080835

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop