Next Article in Journal
Performance Optimization of Polymer Fibre Actuators for Soft Robotics
Next Article in Special Issue
Role of Nanoparticle–Polymer Interactions on the Development of Double-Network Hydrogel Nanocomposites with High Mechanical Strength
Previous Article in Journal
Qualification of New Methods for Measuring In Situ Rheology of Non-Newtonian Fluids in Porous Media
Previous Article in Special Issue
Effect of Various Surface Treatments on the Performance of Jute Fibers Filled Natural Rubber (NR) Composites
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effect of Na2CO3 on the Microstructure and Macroscopic Properties and Mechanism Analysis of PVA/CMC Composite Film

1
School of Material Science and Engineering, East China University of Science and Technology, 130 Meilong Rd, Shanghai 200000, China
2
Shanxi Novofluo New Material Science and Technology Co., LTD, Jinzhong 030600, China
*
Author to whom correspondence should be addressed.
Polymers 2020, 12(2), 453; https://doi.org/10.3390/polym12020453
Submission received: 18 December 2019 / Revised: 11 February 2020 / Accepted: 12 February 2020 / Published: 14 February 2020
(This article belongs to the Collection Reinforced Polymer Composites)

Abstract

:
Polyvinyl alcohol (PVA)/carboxyl methyl cellulose sodium (CMC)/Na2CO3 composite films with different contents of Na2CO3 were prepared by blending and solution-casting. The effect of Na2CO3 on the microstructure of PVA/CMC composite film was analyzed by Fourier-transform infrared (FTIR) spectroscopy, X-ray diffraction (XRD), differential scanning calorimetry (DSC), and atomic force microscopy (AFM). Its macroscopic properties were analyzed by water sorption, solubility, and dielectric constant tests. The results show that the microstructure of PVA/CMC/Na2CO3 composite films was different from that of PVA and PVA/CMC composite films. In addition, compared to PVA and PVA/CMC composite films, the water sorption of PVA/CMC/Na2CO3 composite films relatively increased, the solubility in water significantly decreased, and the dielectric properties significantly improved. All these results indicate that the hydrogen bonding interaction between PVA and CMC increased and the crystallinity of PVA decreased after the addition of Na2CO3. This was also a direct factor leading to increased water sorption, decreased solubility, and enhanced dielectric properties. The reaction mechanism of PVA, CMC, and Na2CO3 is proposed to further evaluate the effect of Na2CO3 on the microstructure and macroscopic properties of PVA/CMC/Na2CO3 composite films.
Keywords:
PVA; CMC; Na2CO3; film

1. Introduction

With increasing difficulties in terms of waste disposal and global warming, severe environmental problems are raising concerns all over the world. In addition, petroleum shortage is also a serious threat throughout the world. Considering these two problems, all countries are trying to develop environmentally friendly materials from nonpetroleum resources. Biopolymers are considered as an ideal alternative to traditional plastic materials owing to their advantages such as biodegradability, nontoxicity, and potential widespread applications; at present, a lot of research is focused on biodegradable materials. Among the biopolymers, cellulose and its water-soluble derivatives are mostly preferred because of the abundance of cellulose on earth and relatively low cost of cellulose derivatives compared to synthetic polymers [1].
Carboxyl methyl cellulose sodium (CMC) is an anionic, linear, and water-soluble polymer; CMC is generally formed by the carboxymethylation of hydroxyl groups in cellulose [2]. CMC has strong water solubility, hydrophilicity, and chemical reactivity because of the presence of hydroxyl and polar carboxylate groups. Moreover, it also has many other characteristic properties such as biocompatibility, renewability, nontoxicity, and biodegradability [3,4,5]. In addition, CMC has many excellent features such as film formation, emulsification, suspension, water retention, and bonding properties. Therefore, it is the most preferred polymer for food, medicine, detergent, paint, paper, flocculant, sizing agent, textile, and other industries [6,7,8,9,10,11]. On the other hand, polyvinyl alcohol (PVA) is a synthetic water-soluble polymer with many applications including textile pulps, adhesives, coatings, dispersants, and a series of medical materials with medical functions owing to its excellent adhesion, flexibility, and film-forming properties [12,13]. PVA is very suitable for blending with natural polymers such as CMC because of its biocompatibility and water solubility [14]. Owing to the presence of hydroxyl groups in both PVA and CMC, stronger intermolecular hydrogen bonds can be formed. Films made from blends of biopolymers generally exhibit more excellent properties compared to films made from biopolymers alone. Therefore, studies on PVA and CMC blend films were a hot topic in recent years. For example, El-Sayed et al. conducted differential scanning calorimetry (DSC), thermogravimetric analysis (TGA), and dielectric spectroscopy of blends of PVA and CMC with different compositions [15]. Zhang et al. controlled the sorption and permeability of PVA/CMC composite films through cross-linking, a potential coating for controlled release of fertilizers [16].
Extensive studies showed that the water sorption and solubility of PVA/CMC composite films have great significance for their applications. At present, some studies showed that different pH environments have a certain effect on the water sorption and solubility of composite films. Ibrahima et al. immersed PVA/CMC and PVA/cellulose composite films in solutions of different pH to evaluate the effect of pH on the solubility of films; the results showed that the solubility of composite films was the lowest at pH 10 [17]. Bajpai et al. studied the swelling ratio of CMC/starch composite films in different pH solutions; the swelling ratio constantly increased with increasing pH [18]. However, these studies only evaluated the water sorption of composite films in different pH solutions, whereas they did not systematically study the microstructure and other macroscopic properties of composite films in different pH solutions.
In this study, PVA and CMC were used as a biopolymer matrix, and Na2CO3 was used as a filler to evaluate its effect on the microscopic and macroscopic properties of PVA/CMC composite films. A reaction mechanism of Na2CO3 with PVA and CMC is proposed, providing a theoretical basis for improving the water sorption, solubility, and dielectric properties of PVA/CMC composite films and promoting their application in biodegradable superabsorbent resins and polymer electrolytes.

2. Materials and Methods

2.1. Materials

PVA (>99%, 87–89% hydrolyzed) and Na2CO3 (99.5%) were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., China. CMC (≥99.5%, Degree of substitution: 0.7) was purchased from Shanghai Yuanye Biotechnology Co., Ltd., China. All chemicals were used as received without any further purification. Deionized water was used, with a conductivity of 0.0556 μs/cm at 25 °C. The structural formula of PVA is as follows:Polymers 12 00453 g010.

2.2. Preparation of Samples

Preparation of PVA/CMC blends: Firstly, a PVA solution was obtained by dissolving 1 g of PVA powder in 19 g of water under stirring at 90 °C for 3 h. Then, 0.4 g of CMC powder was dissolved in 19.6 g of water under stirring at 60 °C for 3 h. Finally, a homogeneous solution of PVA/CMC (2.5/1 w/w) was obtained by adding the CMC solution to the PVA solution and stirring at 85 °C for 3 h.
Preparation of PVA/CMC/Na2CO3 blends: Firstly, a PVA/Na2CO3 blend was obtained by adding an Na2CO3 solution to a PVA solution under stirring at 85 °C for 1 h. The mass of Na2CO3 was varied as 8 wt.%, 12 wt.%, and 16 wt.% of PVA. Then, a PVA/CMC/Na2CO3 solution was obtained by adding the CMC solution to the PVA/Na2CO3 solution under stirring at 85 °C for 3 h.
Preparation of composite films: Firstly, the obtained PVA, PVA/CMC, PVA/Na2CO3, and PVA/CMC/Na2CO3 film-forming solutions were ultrasonicated for 30 min. Next, films were prepared from these solutions on petri dishes using a solution-casting technique. Finally, the cast films were dried at 60 °C for 24 h. The formulations and abbreviations of the samples are shown in Table 1.

2.3. Fourier-Transform Infrared (FTIR) Spectroscopy

FTIR spectra were measured using a NICOLET 6700 spectrometer (Thermo Scientific Co., Waltham, MA, USA) from 4000 cm−1 to 400 cm−1 to study the interaction between PVA and CMC. Samples were ground into powder after drying.

2.4. X-ray Diffraction (XRD)

XRD analysis was carried out using a PANalytical X’Pert-Pro MPD (Almelo, The Netherlands) diffractometer with Cu-Kα radiation (λ = 1.5406 Å) to characterize the crystal form and crystallinity of samples. The diffraction angle ranged from 5° to 80°. Meanwhile, XRD deconvolution analysis was performed using Origin 9.0 software in order to deconvolute specific regions (crystals or amorphous peaks).

2.5. Differential Scanning Calorimetry (DSC)

Thermal properties were measured by DSC using a Netzsch PC200 instrument (Netzsch Inc., Selb, Germany). Specimens weighing 6–9 mg were heated at a rate of 10 °C/min from 25 °C to 250 °C under N2 gas purging.

2.6. Atomic Force Microscopy (AFM) Studies

The morphology of composite films was observed using an atomic force microscope (Veeco, DI) operated in contact mode in air. The test specimen had dimensions of approximately 1.0 mm × 5.0 mm × 5.0 mm (thickness × width × length).

2.7. Dielectric Properties

The dielectric properties were analyzed using a broad-peak dielectric spectrometer (Concept 40, Novocontrol, Montabaur, Germany) in the frequency range from 10−1 to 107 Hz at room temperature. Specimens in the form of a disc of size 30 mm × 2 mm (diameter × thickness) were cut from the dried films.

2.8. Water Sorption

Firstly, the films were weighed (W1) and placed in 90% humidity at room temperature. Then, the films were periodically removed and weighed (W2). The experiment was repeated twice, and the average weight was determined. The water sorption was calculated as follows [19]:
Water sorption = [(W2W1) × 100%]/W1.

2.9. Solubility

Film solubility was determined using the following method: pieces of each film were firstly weighed (W1) and then immersed in deionized water at room temperature for 24 h. Next, the films were taken out and dried in an oven at 60 °C to constant weight (W2). The experiment was repeated twice, and the average weight was determined. The solubility was calculated using Equation (2) [20].
Solubility = [(W1W2) × 100%]/W1.

3. Results and Discussion

3.1. FTIR Spectroscopy

Figure 1 shows the FTIR spectra of PVA, CMC, P/C, P/N, P/C/N, and Na2CO3. For pure PVA, the peaks at 3588 cm−1 and 1330 cm−1 were assigned to OH stretching and bending vibrations for PVA film [21,22]. The peak corresponding to methylene group (CH2) asymmetric stretching vibration appeared at −2932 cm−1 [23]. The peak at −1727 cm−1 corresponded to the C=O symmetrical stretching vibration of the unhydrolyzed ester functional group present on the PVA backbone, and the peak at −1249 cm−1 could be attributed to the C–O–C asymmetric stretching vibration of the ester group [24,25]. For CMC, a strong broad peak was observed at 3541 cm−1, which arose from OH stretching vibration [26]. The vibrational peak observed at 2915 cm−1 could be ascribed to CH asymmetric stretching [24]. The peak at 1607 cm−1 could be attributed to the asymmetric modes of stretching vibration of ester groups (COO) [26]. Two absorption peaks that appeared in the region of 1417 cm−1 and 1325 cm−1 corresponded to scissoring CH2 and bending OH, respectively [27]. For Na2CO3, the peaks at 1426 cm−1, 878 cm−1, and 700 cm−1 were carbonate bands [28]. For P/C/N and P/N composite films, the absorption peaks at 878 cm−1 and 700 cm−1 indicated the presence of Na2CO3. The Na2CO3 absorption peak at 1426 cm−1 was not obvious, because it overlapped with the PVA absorption peak.
The FTIR spectra were analyzed based on two potential regions in Figure 2 in the following ranges of wavenumbers: (a) 3750–2750 cm−1 and (b) 2000–1000 cm−1. The spectrum of the P/C composite film exhibited, in general, the same peaks as those observed in the PVA and CMC films, indicating that no reaction occurred between PVA and CMC [29]. For P/C/N composite films, the absorption peak of OH of PVA moved further toward lower energies than those of the P/C film, exhibiting a shift from 3588 cm−1 to 3464 cm−1. The COO peak of CMC had a similar trend, shifting from 1607 cm−1 to1578 cm−1. At the same time, Figure 2b shows that the OH bending vibration peak of PVA and CMC was gradually weakened with the addition of Na2CO3. The changes in OH stretching vibration peak, OH bending vibration peak, and COO asymmetric stretching vibration indicated an enhancement of hydrogen bonding between PVA and CMC after the addition of Na2CO3, and the intensity of the absorption peak of C=O (1727 cm−1) of PVA gradually decreased with the increase in Na2CO3 content, which could be attributed to the hydrolysis of vinyl acetate group of PVA in an alkaline environment. The acetate group was replaced with a hydroxyl group and, thus, the absorption of C=O of the acetate group in PVA was reduced, as shown in Equation (3). The intensity of the absorption peak of the methylene group (CH2) for the P/C/N3 composite film was significantly reduced. Because OH is an electron-donating group, the electron cloud density around the C atom connecting the hydroxyl group was increased, and the electron cloud density around the C atom adjacent to the methylene group was affected, thus decreasing the absorption peak intensity of methylene group. For the P/N3 composite film, the absorption peak of OH moved to 3475 cm−1, which was related to the formation of intermolecular hydrogen bonds in PVA. The disappearance of the C=O absorption peak in the spectrum of the P/N3 composite film confirmed the reaction shown in Equation (3).
Polymers 12 00453 g011

3.2. XRD Analysis

The XRD patterns of PVA, CMC, P/C, P/N, P/C/N, and Na2CO3 are shown in Figure 3. The crystallinity (Xc) of the obtained films was determined from the equation Xc = Ac/(Ac + Aa) × 100 (where Ac and Aa are the peak intensities of crystalline and amorphous cellulose, respectively) [30]. The results are shown in Table 2. Figure 3 shows that pure PVA had two sharp diffraction peaks at 19.7° and 40.8° corresponding to an orthorhombic lattice (110) reflection [31]. On the other hand, three diffraction peaks for pure CMC appeared at 20.7°, 31.8°, and 45.7°. Compared to pure PVA and CMC films, the position of the diffraction peak of the P/C composite film had no obvious movement. This indicated that there was no new crystal form, but the crystallinity of the P/C composite film compared to that of the PVA film was reduced, probably because the CMC macromolecular chains inhibited the movement of the PVA molecular chains [32]. For the P/N3 film, the crystallinity was significantly weakened compared to PVA, indicating that the addition of Na2CO3 destroyed the crystal structure of PVA. After adding CMC, the crystallinity of the P/C/N composite films continued to decrease. This was related to the hindrance of the CMC macromolecular chain. However, Figure 3 and Table 2 show no significant change in the peak position and crystallinity of P/C/N composite films compared to those of the P/C film. Considering that this was related to the use of Na2CO3 as a nucleating agent, the crystallinity of P/C/N composite films was improved. Figure 3 also shows that the XRD peak corresponding to crystalline Na2CO3 was not obvious in composite films; however, it can be speculated that the crystallinity of Na2CO3 in the composite films was greatly reduced [33,34].

3.3. DSC Analysis

Figure 4 shows the characteristic features of the DSC curves for the studied composite films. The crystallinity of composite films could be calculated using the formula Xc = (ΔH/wΔHc) × 100%), where ΔHc = 161 J/g, and w is the mass fraction of PVA in the composite films [35]. The results are shown in Table 3. The crystallinity obtained from DSC was different from that obtained from XRD, but the trend of crystallinity changes was completely consistent. For the PVA film, DSC showed an endotherm melting transition at 192 °C, representing the melting temperature of PVA. The DSC thermogram of P/C showed an endotherm melting transition at 178 °C, lower than that of PVA. The melting temperature decreased due to a decrease in the crystallinity degree, consistent with the XRD and DSC results.
The P/C/N1 composite film exhibited an endotherm melting transition at 194 °C, which was higher than the melting temperature of PVA, and the crystallinity degree of the film was lower than that of PVA. This was because of an increase in the intermolecular hydrogen bonds of PVA and CMC, as indicated by the FTIR results. The hydrogen bonds between PVA and CMC inhibited the movement of PVA molecular chains, increasing the melting temperature and decreasing the crystallinity degree of P/C/N composite films. This also showed that the melting temperature of the P/C/N composite films increased with the increasing content of Na2CO3. This was because the crystal structure of PVA was gradually destroyed as the content of Na2CO3 increased. The PVA molecular chains became disordered, which strengthened the contact of PVA and CMC. At the same time, as Na2CO3 content increased, more ester groups were hydrolyzed, and the amount of hydroxyl groups increased. This generated more intermolecular hydrogen bonds and, thus, increased the melting temperature. Moreover, the crystallinity of the P/C/N composite films was higher than that of P/C composite film, consistent with the XRD results. At the same time, the crystallinity of the P/C/N composite films gradually increased with the increase in sodium carbonate content, which was also related to the role of sodium carbonate as a nucleating agent.

3.4. Dielectric Analysis

Figure 5 shows the patterns of dielectric constant as a function of frequency at room temperature for the resulting composite films. In general, the dielectric constant of pure PVA was low, and the dielectric constant of the P/C composite film was slightly increased. However, the dielectric constant of P/C/N composite films was significantly improved with the addition of Na2CO3, and it also gradually increased with increasing Na2CO3 content. Specially, the dielectric constant of the P/C/N3 composite film was 32,000 at 102 Hz, 25 times higher than that of the P/C composite film (the dielectric constant of the P/C composite film was 1210 at 102 Hz). This could be ascribed to the addition of Na2CO3, which promoted the generation of hydrogen bonds between PVA and CMC molecules. This led to a multimolecular dipole, significantly increasing the dielectric constant of P/C/N composite films.
At the same time, the dielectric constant of pure PVA slightly varied with frequency and remained constant. The change in dielectric constant for the P/C composite film was also very small. However, the dielectric constants of P/C/N composite films rapidly decreased with increasing frequency in the low-frequency range, while they decreased very slowly when the frequency was above 105 Hz. This was because, with the addition of Na2CO3, the composite films had a certain dielectric relaxation phenomenon in the low-frequency range, and this phenomenon was gradually attenuated in the high-frequency range [36].

3.5. Water Sorption Analysis

Figure 6 shows the water sorption of PVA, P/C, and P/C/N composite films, which were significantly different. The pure PVA film exhibited the lowest water sorption. For the P/C composite film, the water sorption ability was higher than that of pure PVA. This was because the actual mixing of two different types of molecules led to the deformation of the structure, making the network more hydrophilic [29]. In addition, the poor water sorption ability of the pure PVA film could be attributed to higher intermolecular attraction and strong intramolecular or intermolecular hydrogen bonding.
The water sorption of P/C/N composite films was significantly higher than that of the pure PVA film, but lower than that of the P/C composite film. This was because the addition of Na2CO3 disrupted the crystal structure of PVA. The molecular chain of PVA changed from regular to disordered. This enhanced the contact with water molecules, making the water sorption of P/C/N composite films significantly higher than that of PVA film. Similar results were reported in the literature [18]. However, it also promoted the formation of hydrogen bonds between PVA and CMC, and the hydrogen bonds acted as a physical crosslinking point, promoting the formation of a much denser molecular structure. Therefore, its water sorption was significantly lower than that of the P/C composite film. The water sorption of the P/C/N2 composite film was lower than that of the P/C/N1 composite film because the hydrogen bonding between PVA and CMC was strengthened with the increase in Na2CO3 content, and a denser molecular structure was formed. The water sorption of the P/C/N3 composite film was slightly increased. This was related to excess Na2CO3, i.e., the PVA molecular chain was in sufficient contact with water molecules. At the same time, excess sodium carbonate also caused the ionization of the carboxyl group of CMC, and the COO/COOH ratio of CMC also increased because of the increasing ionization of carboxylic groups. This resulted in a greater mutual repulsion among the COO-bearing CMC chains, consequently causing the CMC chains to undergo faster relaxation. This widened the mesh sizes of free volumes, resulting in a larger water sorption ratio [37].

3.6. Solubility Analysis

Figure 7 shows the solubility of PVA, P/C, P/C/N1, P/C/N2, and P/C/N3 composite films. Compared to the PVA film and P/C composite film, the solubility of the P/C/N composite films was significantly reduced with the addition of Na2CO3, further confirming the formation of intermolecular hydrogen bonding. The P/C/N2 composite film showed the lowest solubility of 24%, slightly lower than the solubility of the P/C/N1 composite film. This indicated that the hydrogen bonding network of the P/C/N2 composite film was denser. This result is similar to that of Ibrahima et al., i.e., the composite film showed the lowest solubility in a certain alkaline environment [17]. The solubility of the P/C/N3 composite film was slightly increased to 25%, which was related to the increased contact between the disordered molecular chains and water molecules. Secondly, the ionization of the CMC carboxyl group increased the mesh size of its free volume, which was also an important factor. A significant decrease in the solubility of the P/C/N composite films indicated that hydrogen bonding was the most important factor affecting the solubility of composite films, and slight changes in the solubility of the P/C/N3 composite film showed that the change in molecular structure also had a certain effect on the solubility of composite films.

3.7. Surface Topography Analysis

The representative images obtained from AFM studies for the studied composite films are shown in Figure 8. Clearly, film surfaces with varying levels of surface roughness were present. The surfaces of the PVA film and P/C composite film were smooth and flat, and the surface of the P/C/N1 composite film was also relatively smooth. As the content of Na2CO3 increased, the surfaces of the P/C/N2 and P/C/N3 composite films became rough and uneven; Table 4 shows the corresponding roughness. According to the results of water sorption, although the roughness of P/C/N2 increased significantly, its water sorption still decreased, indicating that the roughness of the surface of composite films had a small effect on water sorption. As the main factors of water sorption, surface roughness, pores, and molecular structure are always mentioned, obviously, no pores were found in the composite films [38]. Thus, the interaction between PVA and CMC under the action of Na2CO3 was proven to be the main factor affecting the water sorption of composite films.

3.8. Mechanism Analysis

FTIR, DSC, XRD, and the dielectric constant test results of P/C/N composite films were significantly different from those of the PVA film and P/C composite film. In addition, the solubility of the P/C/N composite films was much lower than that of the PVA film and P/C composite film, indicating the formation of a crosslinking structure in P/C/N composite films. The water sorption of the P/C/N composite films was higher than that of the PVA film, but lower than that of the P/C composite film, indicating that Na2CO3 promoted the relaxation of the PVA and CMC structure. Based on the above information, a reaction mechanism is proposed for Na2CO3, PVA, and CMC.
Na2CO3 is alkaline in water and ionizes OH groups. At a certain temperature (80 °C), the alkali can hydrolyze the vinyl acetate group in the partially alcoholic PVA; the acetate group is replaced with a hydroxyl group. The amount of hydroxyl groups in PVA increases, consistent with the weakening C=O absorption peak of P/C/N and P/N composite films in the FTIR spectrum. At the same time, the crystal structure of PVA is significantly destroyed in an alkaline environment, consistent with the XRD results of P/N film. The destruction of the crystal structure of PVA further stretches the molecular chain of PVA and strengthens the contact with the molecular chain of CMC, thus promoting the formation of intermolecular hydrogen bonds between the OH and COOH groups of CMC and the OH group of PVA. The shift in C=O and OH characteristic absorption peaks, the decrease in crystallinity, the increase in the melting point, and the increase in dielectric constant indicate the formation of intermolecular hydrogen bonds between PVA and CMC, as shown in Figure 9. In addition, the stretching of the PVA molecular chain enhances its contact with water molecules; the ionization of the CMC carboxyl group leads to an increase in the mesh size of its free volume, significantly increasing the water sorption of P/C composite films doped with Na2CO3. However, the increase in hydrogen bonding between PVA and CMC makes the molecular structure denser, which is the main reason for the decrease in water sorption and solubility.

4. Conclusions

This study shows that Na2CO3 significantly affected the microstructure and macroscopic properties of P/C/N composite films. FTIR, XRD, AFM, DSC, and dielectric properties confirmed that Na2CO3 promoted the formation of intermolecular hydrogen bonds between PVA and CMC. The water sorption and solubility tests showed that the composite films had reasonable water sorption capacity and water-resisting properties, resulting from the synergistic interaction between the relaxation of the molecular chain and intermolecular hydrogen bonding between PVA and CMC. This study showed how the salt affects the microstructure and macroscopic properties of composite films. This has long-term significance in promoting the application of biodegradable superabsorbent resins and polymer electrolytes.

Author Contributions

Data curation, J.Z.; formal analysis, J.Z.; investigation, J.Z., X.L., C.D., X.C. and C.W.; methodology, J.Z.; project administration, Q.L. and Y.C.; writing—original draft, J.Z.; writing—review and editing, Q.L. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Vlaia, L.; Coneac, G. Cellulose-derivatives-based hydrogels as vehicles for dermal and transdermal drug delivery. Emerg. Concepts Anal. Appl. Hydrogels 2016. [Google Scholar] [CrossRef] [Green Version]
  2. Kumar:, B.; Negi, Y.S. Water absorption and viscosity behaviour of thermally stable novel graft copolymer of carboxymethyl cellulose and poly(sodium 1-hydroxy acrylate). Carbohydr. Polym. 2018, 181, 862–870. [Google Scholar] [CrossRef] [PubMed]
  3. Entcheva, E.; Bien, H.; Yin, L.; Chung, C.Y.; Farrell, M.; Kostov, Y. Functional cardiac cell constructs on cellulose-based scaffolding. Biomaterials 2004, 25, 5753–5762. [Google Scholar] [CrossRef] [PubMed]
  4. Liu, H.; Huang, S.; Li, X.; Zhang, L.; Tan, Y.; Wei, C.; Lv, J. Facile fabrication of novel polyhedral oligomeric silsesquioxane/carboxymethyl cellulose hybrid hydrogel based on supermolecular interactions. Mater. Lett. 2013, 90, 142–144. [Google Scholar] [CrossRef]
  5. Saha, N.; Shah, R.; Gupta, P.; Mandal, B.B.; Alexandrova, R.; Sikiric, M.D.; Saha, P. PVP-CMC hydrogel: An excellent bioinspired and biocompatible scaffold for osseointegration. Mater. Sci. Eng. 2019, 95, 440–449. [Google Scholar] [CrossRef]
  6. Agbovi, H.K.; Wilson, L.D. Design of amphoteric chitosan flocculants for phosphate and turbidity removal in wastewater. Carbohydr. Polym. 2018, 189, 360–370. [Google Scholar] [CrossRef]
  7. Holder, M.K.; Peters, N.V.; Whylings, J.; Fields, C.T.; Gewirtz, A.T.; Chassaing, B.; de Vries, G.J. Dietary emulsifiers consumption alters anxiety-like and social-related behaviors in mice in a sex-dependent manner. Sci. Rep. 2019, 9, 172. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  8. Mishra, S.; Usha Rani, G.; Sen, G. Microwave initiated synthesis and application of polyacrylic acid grafted carboxymethyl cellulose. Carbohydr. Polym. 2012, 87, 2255–2262. [Google Scholar] [CrossRef]
  9. Toǧrul, H.; Arslan, N. Carboxymethyl cellulose from sugar beet pulp cellulose as a hydrophilic polymer in coating of mandarin. J. Food Eng. 2004, 62, 271–279. [Google Scholar] [CrossRef]
  10. Yang, Y.; Wang, R.; Feng, W.; Zhou, X.; Chen, Z.; Wang, T. Carboxymethylcellulose/pectin inhibiting structural folding of rice proteins via trinary structural interplays. Int. J. Biol. Macromol. 2019, 133, 93–100. [Google Scholar] [CrossRef]
  11. Zhang, T.; Wang, Y.; Luo, G.; Bai, S. Preparation of highly dispersed precipitated nanosilica in a membrane dispersion microreactor. Chem. Eng. J. 2014, 258, 327–333. [Google Scholar] [CrossRef]
  12. Harazono, K.; Nakamura, K. Decolorization of mixtures of different reactive textile dyes by the white-rot basidiomycete Phanerochaete sordida and inhibitory effect of polyvinyl alcohol. Chemosphere 2005, 59, 63–68. [Google Scholar] [CrossRef] [PubMed]
  13. Zhu, Y.; Yu, X.; Zhang, T.; Wang, X. Constructing zwitterionic coatings on thin-film nanofibrous composite membrane substrate for multifunctionality. Appl. Surf. Sci. 2019, 483, 979–990. [Google Scholar] [CrossRef]
  14. Follain, N.; Joly, C.; Dole, P.; Bliard, C. Properties of starch based blends. Part 2. Influence of poly vinyl alcohol addition and photocrosslinking on starch based materials mechanical properties. Carbohydr. Polym. 2005, 60, 185–192. [Google Scholar] [CrossRef]
  15. El-Sayed, S.; Mahmoud, K.H.; Fatah, A.A.; Hassen, A. DSC, TGA and dielectric properties of carboxymethyl cellulose/polyvinyl alcohol blends. Phys. B Condens. Matter 2011, 406, 4068–4076. [Google Scholar] [CrossRef]
  16. Zhang, L.; Zhang, G.; Lu, J.; Liang, H. Preparation and characterization of carboxymethyl cellulose/polyvinyl alcohol blend film as a potential coating material. Polym.-Plast. Technol. Eng. 2013, 52, 163–167. [Google Scholar] [CrossRef]
  17. Ibrahim, M.M.; Koschella, A.; Kadry, G.; Heinze, T. Evaluation of cellulose and carboxymethyl cellulose/poly(vinyl alcohol) membranes. Carbohydr. Polym. 2013, 95, 414–420. [Google Scholar] [CrossRef]
  18. Bajpai, A.K.; Shrivastava, J. In vitro enzymatic degradation kinetics of polymeric blends of crosslinked starch and carboxymethyl cellulose. Polym. Int. 2005, 54, 1524–1536. [Google Scholar] [CrossRef]
  19. Paralikar, S.; Simonsen, J.; Lombardi, J. Poly(vinyl alcohol)/cellulose nanocrystal barrier membranes. J. Membr. Sci. 2008, 320, 248–258. [Google Scholar] [CrossRef]
  20. Sivakumar, M.; Malaisamy, R.; Sajitha, C.J.; Mohan, D. Preparation and performance of cellulose acetate–polyurethane blend membranes and their applications—II. J. Membr. Sci. 2000, 169, 215–228. [Google Scholar] [CrossRef]
  21. El-Sawy, N.M.; El-Arnaouty, M.B.; Ghaffar, A.M.A. γ-Irradiation effect on the non-cross-linked and cross-linked polyvinyl alcohol films. Polym.-Plast. Technol. Eng. 2010, 49, 169–177. [Google Scholar] [CrossRef]
  22. Dai, H.; Huang, Y.; Huang, H. Eco-friendly polyvinyl alcohol/carboxymethyl cellulose hydrogels reinforced with graphene oxide and bentonite for enhanced adsorption of methylene blue. Carbohydr. Polym. 2017, 185, 1–11. [Google Scholar] [CrossRef] [PubMed]
  23. Houssein, A.; Claude, D. Chemical modification of poly(vinyl alcohol) in water. Appl. Sci. 2015, 5, 840–850. [Google Scholar]
  24. Kuanova, A.; Nurpeissova, Z.A.; Mangazbayeva, R.; Park, K. The obtaining of composite materials based on carboxymethylcellulose and polyvinyl alcohol. Int. J. Biol. Chem. 2017, 10, 62–68. [Google Scholar] [CrossRef]
  25. Mansur, H.S.; Sadahira, C.M.; Souza, A.N.; Mansur, A.A. FTIR spectroscopy characterization of poly (vinyl alcohol) hydrogel with different hydrolysis degree and chemically crosslinked with glutaraldehyde. Mater. Sci. Eng. C 2008, 28, 539–548. [Google Scholar] [CrossRef]
  26. Zhu, Y.; Xiao, S.; Li, M.; Chang, Z. Natural macromolecule based carboxymethyl cellulose as a gel polymer electrolyte with adjustable porosity for lithium ion batteries. Power Sources 2015, 288, 368–375. [Google Scholar] [CrossRef]
  27. Biswal, D.; Singh, R. Characterisation of carboxymethyl cellulose and polyacrylamide graft copolymer. Carbonhydrate Polym. 2004, 57, 379–387. [Google Scholar] [CrossRef]
  28. Mei, Y.; Wang, Z.; Fang, H. Na-containing mineral transformation behaviors during Na2CO3-catalyzed CO2 gasification of high-alumina coal. Energy Fuels 2017, 31, 1235–1242. [Google Scholar] [CrossRef]
  29. Lagarón, J.M.; López-Rubio, A.; José Fabra, M. Bio-based packaging. J. Appl. Polym. Sci. 2016, 133. [Google Scholar] [CrossRef]
  30. Zainuddin, N.K.; Samsudin, A.S. Investigation on the effect of NH4Br at transport properties in k–carrageenan based biopolymer electrolytes via structural and electrical analysis. Mater. Today Commun. 2018, 14, 199–209. [Google Scholar] [CrossRef]
  31. Alakanandana, A.; Subrahmanyam, A.R.; Siva Kumar, J. Structural and electrical conductivity studies of pure PVA and PVA doped with succinic acid polymer electrolyte system. Mater. Today Proc. 2016, 3, 3680–3688. [Google Scholar] [CrossRef]
  32. El-Gamal, S.; El Sayed, A.M.; Abdel-Hady, E.E. Effect of cobalt oxide nanoparticles on the nano-scale free volume and optical properties of biodegradable CMC/PVA films. J. Polym. Environ. 2017, 26, 2536–2545. [Google Scholar] [CrossRef]
  33. Uthayakumar, A.; Pandian, A.; Mathiyalagan, S. Interfacial effect of the oxygen-ion distribution on the conduction mechanism in strontium-added Ce0.8Sm0.2O2-δ/Na2CO3 nanocomposite. Phys. Chem. 2016, 120, 25068–25077. [Google Scholar] [CrossRef]
  34. Raza, R.; Wang, X.; Ma, Y.; Liu, X.; Zhu, B. Improved ceria-carbonate composite electrolytes. Hydrog. Energy 2010, 35, 2684–2688. [Google Scholar] [CrossRef]
  35. Blaine, R.L. Thermal applications note. TN 48. In Polymer Heats of Fusion; TA Instrument: New Castle, DE, USA, 2002. [Google Scholar]
  36. El-Zawawy, W.K. Blended graft copolymer of carboxymethyl cellulose and poly(vinyl alcohol) with banana fiber. J. Appl. Polym. Sci. 2006, 100, 1842–1848. [Google Scholar] [CrossRef]
  37. Peppas, N.A.; Wright, S.L. Solution diffusion in poly[(vinyl alcohol)/poly(acrylic acid)] interpenetrating networks. Macromolecules 1996, 29, 8798–8804. [Google Scholar] [CrossRef]
  38. Baig, M.I.; Ingole, P.G.; Jeon, J.-D.; Hong, S.U.; Choi, W.K.; Jang, B.; Lee, H.K. Water vapor selective thin film nanocomposite membranes prepared by functionalized silicon nanoparticles. Desalination 2019, 451, 59–71. [Google Scholar] [CrossRef]
Figure 1. Fourier-transform infrared (FTIR) spectra of Na2CO3 and the obtained composite films.
Figure 1. Fourier-transform infrared (FTIR) spectra of Na2CO3 and the obtained composite films.
Polymers 12 00453 g001
Figure 2. FTIR spectra of Na2CO3 and the obtained composite films: (a) region from 3750 cm−1 to 2750 cm−1; (b) region from 2000 cm−1 to 1000 cm−1.
Figure 2. FTIR spectra of Na2CO3 and the obtained composite films: (a) region from 3750 cm−1 to 2750 cm−1; (b) region from 2000 cm−1 to 1000 cm−1.
Polymers 12 00453 g002
Figure 3. X-ray diffraction (XRD) patterns of Na2CO3 and the obtained composite films.
Figure 3. X-ray diffraction (XRD) patterns of Na2CO3 and the obtained composite films.
Polymers 12 00453 g003
Figure 4. Differential scanning calorimetry (DSC) curves of the obtained composite films.
Figure 4. Differential scanning calorimetry (DSC) curves of the obtained composite films.
Polymers 12 00453 g004
Figure 5. The dielectric constants of the obtained composite films at (a) low frequency and (b) high frequency.
Figure 5. The dielectric constants of the obtained composite films at (a) low frequency and (b) high frequency.
Polymers 12 00453 g005
Figure 6. Water sorption of PVA, P/C, P/C/N1, P/C/N2, and P/C/N3 composite films.
Figure 6. Water sorption of PVA, P/C, P/C/N1, P/C/N2, and P/C/N3 composite films.
Polymers 12 00453 g006
Figure 7. Solubility of the obtained composite films.
Figure 7. Solubility of the obtained composite films.
Polymers 12 00453 g007
Figure 8. Representative atomic force microcopy (AFM) images of (a) PVA, (b) P/C, (c) P/C/N1, (d) P/C/N2, and (e) P/C/N3 composite films.
Figure 8. Representative atomic force microcopy (AFM) images of (a) PVA, (b) P/C, (c) P/C/N1, (d) P/C/N2, and (e) P/C/N3 composite films.
Polymers 12 00453 g008
Figure 9. The reaction mechanism for PVA, CMC, and Na2CO3.
Figure 9. The reaction mechanism for PVA, CMC, and Na2CO3.
Polymers 12 00453 g009
Table 1. The formulations and abbreviations of the samples. PVA—polyvinyl alcohol; CMC—carboxyl methyl cellulose sodium.
Table 1. The formulations and abbreviations of the samples. PVA—polyvinyl alcohol; CMC—carboxyl methyl cellulose sodium.
SampleSample NotationPVA SolutionCMC SolutionNa2CO3 Solution
PVA (g)Water (g)CMC (g)Water (g)Na2CO3 (g)Water (g)
PVAPVA119
CMCCMC 0.419.6
PVA/CMCP/C1190.419.6
PVA/CMC/Na2CO3P/C/N11190.419.60.085
P/C/N21190.419.60.125
P/C/N31190.419.60.165
PVA/Na2CO3P/N3119 0.165
Table 2. Percentage of crystallinity of the obtained composite films.
Table 2. Percentage of crystallinity of the obtained composite films.
SampleAcAaXc (%)
PVA2270422334.96
CMC373183417.65
P/C12415367.47
P/C/N321495318.34
P/N3501197920.20
Table 3. DSC data for the obtained composite films.
Table 3. DSC data for the obtained composite films.
SamplePVAP/CP/C/N1P/C/N2P/C/N3
Tm (°C)192178194200212
Melting enthalpy (J/g)33.838.9416.1824.8725.50
Crystallinity (%)21.017.7714.8723.4824.71
Table 4. Roughness of the obtained composite films.
Table 4. Roughness of the obtained composite films.
PVAP/CP/C/N1P/C/N2P/C/N3
Rq10.20519.96316.160295.52264.09
Ra7.75615.11511.991233.14210.62

Share and Cite

MDPI and ACS Style

Zhu, J.; Li, Q.; Che, Y.; Liu, X.; Dong, C.; Chen, X.; Wang, C. Effect of Na2CO3 on the Microstructure and Macroscopic Properties and Mechanism Analysis of PVA/CMC Composite Film. Polymers 2020, 12, 453. https://doi.org/10.3390/polym12020453

AMA Style

Zhu J, Li Q, Che Y, Liu X, Dong C, Chen X, Wang C. Effect of Na2CO3 on the Microstructure and Macroscopic Properties and Mechanism Analysis of PVA/CMC Composite Film. Polymers. 2020; 12(2):453. https://doi.org/10.3390/polym12020453

Chicago/Turabian Style

Zhu, Jufang, Qiuying Li, Yanchao Che, Xingchen Liu, Chengcheng Dong, Xinyu Chen, and Chao Wang. 2020. "Effect of Na2CO3 on the Microstructure and Macroscopic Properties and Mechanism Analysis of PVA/CMC Composite Film" Polymers 12, no. 2: 453. https://doi.org/10.3390/polym12020453

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop