3.1. IR Spectra of the Copolymer PMEuTb
The infrared spectra of the complexes Eu(TTA)
2(phen)UA and Tb(p-BBA)
3UA, and polymers PMMA and PMEuTb, were recorded by the KBr tablet method, as shown in
Figure 2. The infrared characteristic data are listed in
Table 1. In the complex Eu(TTA)
2(phen)UA, 1242, 1190 and 1138 cm
−1 belong to the antisymmetric and symmetric stretching vibration multiplets of CF
3 in the ligand TTA, the peak at 1588 cm
−1 is attributed to the stretching vibration of C=O in TTA redshifts to 1600 cm
−1 in the complex and the characteristic peak at 493 cm
−1 is assigned to the stretching vibration of Eu-O, indicating that the C=O in TTA has coordinated with the Eu(III) ions. The peak at 1462 cm
−1 is assigned to the stretching vibration of C=N in the ligand phen, and the weak absorption peak at 460 cm
−1 belongs to the stretching vibration of Eu-N, indicating that phen has coordinated with the Eu(III) ions. The peaks at 1535 cm
−1 and 1413 cm
−1 assigned to the antisymmetric and symmetric stretching vibration of carboxylate COO- are detected in the complex, owing to the loss of H
+ ions from -COOH, indicating that UAH coordinates successfully with the Eu(III) ions.
It can be seen from the infrared spectra of the complex Tb(p-BBA)3UA that the peak at 1591 cm−1 is attributed to the stretching vibration of carbonyl C=O from the ligand p-BBA, the stretching vibration peaks of C=O at 1680 cm−1 and C-O at 1289 cm−1 in the ligand both disappear in the complex, the antisymmetric and symmetric stretching vibration of carboxylate COO- are probed at 1543 cm−1 and 1417 cm−1 and the characteristic peak at 495 cm−1 is assigned to the stretching vibration of Tb-O. The results indicate that the ligand p-BBA has coordinated with the Tb(III) ions. The C=C stretching vibration frequency is detected at 1654 cm−1, indicating that UAH has coordinated with the Tb(III) ions.
As can be seen from
Figure 2, homopolymer PMMA has a similar infrared spectrum to copolymer PMEuTb. In the copolymer PMEuTb, the antisymmetric and symmetric stretching vibration peaks of CH
3 are located at 2999 cm
−1 and 2953 cm
−1, the asymmetric and symmetric variable angle vibration peaks are located at 1479 cm
−1 and 1446 cm
−1 and the characteristic absorption peak at 1732 cm
−1 is assigned to the stretching vibration peak of ester carbonyl C=O. It should be noted that the characteristic peaks of the complexes were not detected in the copolymer PMEuTb, in that the content of the complexes was low (<5%).
3.2. UV-vis Absorption Spectra of the Copolymer PMEuTb
The UV-vis absorption spectra of Eu(TTA)
2(phen)UA, Tb(
p-BBA)
3UA, TTA, phen,
p-BBA, PMMA and PMEuTb were measured using dimethyl sulfoxide as a solvent at a concentration of 1 × 10
−4 mol/L, as shown in
Figure 3. It can be seen that there are mainly three absorption peaks in the complex Eu(TTA)
2(phen)UA. The absorption peaks at 210, 230 and 254 nm in the free ligand phen are attributed to the π-π* transition and
n-π* transition of biphenyl structure. The absorption peak at 230 nm in the ligand phen redshifts to 233 nm in the complex. The two absorption peaks at 280 nm and 354 nm in the complex belong to the absorption of the ligand TTA at 264, 290 and 337 nm. However, compared with the ligand TTA, the absorption peaks generate redshift in the complex, which is caused by the formation of a larger conjugate system after the formation of the complex. From the complex Tb(
p-BBA)
3UA, it is clear that the absorption peak at 240~322 nm in the ligand p-BBA redshifts to 244~330 nm in the complex Tb(
p-BBA)
3UA, which is caused by the formation of a larger conjugate system after the formation of the complex. The weak peak at 231 nm belongs to B absorption band of the benzene ring in the ligand
p-BBA. Since the ligand UA is an aliphatic compound, it does not contain rigid groups such as benzene rings, and has poor light absorption ability, so it does not show the absorption of UAH in the complexes.
Compared with the homopolymer PMMA, after the introduction of the complexes Eu(TTA)
2(phen)UA and Tb(
p-BBA)
3UA, the UV-vis absorption spectrum of the obtained copolymer PMEuTb shows not only the absorption of polymer matrix PMMA, but also the absorption of the two complexes. The overall peak shape of the copolymer PMEuTb is similar to that of PMMA. However, the intensity of the absorption peak at 275 nm is significantly enhanced, which is represented by the junction absorption of Tb(p-BBA)
3UA, Eu(TTA)
2(phen)UA and PMMA. The intensity at 365 nm is also enhanced, which is attributed to the absorption of the complex Eu(TTA)
2(phen)UA and PMMA. These results indicate that the complexes Eu(TTA)
2(phen)UA and Tb(p-BBA)
3UA have copolymerized with methyl methacrylate to form copolymer PMEuTb. It was further proved that, by introducing a small amount of complex monomer, the copolymer shows strong UV absorption characteristic peaks of the complexes and the position of the characteristic peaks remain, indicating that the complex not only participates in the copolymerization, but also is difficult to dissociate after polymerization [
25]. At the same time, it also proves the correctness of inference that the complex monomers are not detected in PMEuTb infrared spectra of
Figure 2 in the low content of the complex monomers.
3.3. Thermal Stability of the Copolymer PMEuTb
The TG curves of Eu(TTA)
2(phen)UA, Tb(p-BBA)
3UA, PMMA and PMEuTb were measured in a dynamic N
2 atmosphere at a rate of 10 °C/min, and the DTG curves were obtained by first-order differentiation of the TG curve, as shown in
Figure 4. It can be learned from the TG curves that the initial decomposition temperature of the complex Eu(TTA)
2(phen)UA is 290 °C, and no mass loss occurs before this temperature, indicating that the complex Eu(TTA)
2(phen)UA does not contain coordination water or water. The weight loss starts from 290 °C, the weight loss rate of the complex is 52% and the maximum weight loss rate occurs at 380 °C. At this stage, the ligands TTA and UA are mainly decomposed, being consistent with the theoretical decomposition rate of 55%. The residue is mainly stable Eu
2O
3.The decomposition of the complex Tb(p-BBA)
3UA can be divided into three stages: The first weight loss stage is before 368 °C, and the weight loss rate of the complex is 1%, indicating that the complex contains trace water by confirming an OH
− characteristic absorption peak at 3400 cm
−1 in the infrared spectra. At the stage of 368~616 °C, the maximum weight loss rate is located at 515 °C, and the weight loss rate at this stage is 39%. This stage is mainly the decomposition of the ligands p-BBA and UAH. After 616 °C, the complex slowly loses 4% of its mass, at which the complex decomposes completely and the remainder is Tb
2O
3.
The thermal property changes of the copolymer PMEuTb are similar to those of the homopolymer PMMA, and can be divided into three stages: In the first stage, the thermal properties are stable before 240 °C and its weight loss is zero due to the little impurity. The initial decomposition temperature of the copolymer PMEuTb increases from 208 °C of the homopolymer to 240 °C, indicating that, after the introduction of complex Eu(TTA)2(phen)UA and Tb(p-BBA)3UA, the rigid groups such as benzene rings are introduced into the side chain of the molecular chain of the copolymer, and the overall rigidity of the molecular chain is improved, leading to the increase of the initial decomposition temperature. The second stage occurs between 240 and 329 °C and the maximum thermal decomposition rate occurs at 314 °C. Compared with 26% weight loss of PMMA, PMEuTb has 19% weight loss, indicating that PMEuTb contains less small molecular polymer. The last stage occurs between 329 and 454 °C, with obvious weight loss, complete decomposition at 454 °C and the maximum decomposition rate at 399 °C. This stage is mainly the depolymerization of high molecular weight PMEuTb “zipper” and the decomposition of complex monomers. Compared with PMMA, the temperature at maximum decomposition rate is increased by 26 °C, indicating that the introduction of complexes is beneficial to improve the thermal stability of PMMA.
3.4. Luminescent Properties of the Complexes Eu(TTA)2(phen)UA and Tb(p-BBA)3UA
The resolution was (1 nm, 1 nm), the monitoring wavelength was 613 nm and the excitation spectrum of the complex Eu(TTA)
2(phen)UA was measured at room temperature, as shown in
Figure 5a. The complex exhibits a broad excitation band of 200~400 nm with 365 nm as the optimal excitation peak. This is due to the fact that the ligands TTA and phen form a large conjugated structure after coordination with the Eu(III) ions, leading to a broad excitation band. The emission spectrum was measured with 365 nm as the excitation wavelength, as presented in
Figure 5a. As can be seen from the figure, the characteristic emissions of Eu(III) ions are detected at 580, 591, 613 and 654 nm, corresponding to
5D
0–
7F
0,
5D
0–
7F
1,
5D
0–
7F
2 and
5D
0–
7F
3 level transitions of the Eu(III) ions, respectively. The
5D
0–
7F
2 transition at 613 nm is the strongest, and the full width at half maximum (FWHM) is less than 5 nm, displaying high color purity. It is due to the fact that the
5D
0–
7F
2 transition is a so-called “hypersensitive transition”, which means that its intensity is much more influenced by the local symmetry of the Eu(III) ions and the nature of the ligands than the intensities of the other electric dipole transitions. The
5D
0–
7F
1 transition at 591 nm is a magnetic dipole-allowed transition, whose intensity is largely independent of the environment of the Eu(III) ions. The emissions at 580 nm and 654 nm are contributed to by the
5D
0–
7F
0 and
5D
0–
7F
3 electric dipole transitions, which are forbidden transitions according to the standard Judd–Ofelt theory, and it is assumed that the two transitions are due to J-mixing [
26]. The luminescence process of the complex Eu(TTA)
2(phen)UA can be explained in terms of energy transfer; the ligands TTA and phen absorb energy, electrons are excited from the ground state to the lowest singlet state, the energy is transferred to the lowest triplet state of the ligand by inter-system leap, then, the energy is transferred from the lowest triplet state of the ligands to the resonance energy level
5D
0 of the Eu(III) ions by electron exchange and the 4f electrons of the Eu(III) ions emit characteristic light when they migrate back to the ground state by radiation.
The resolution was (1 nm, 1 nm) and the excitation spectrum of the complex Tb(p-BBA)
3UA was measured and monitored at 545 nm, as illustrated in
Figure 5b. The complex exhibits strong excitation bands between 200 and 400 nm with 280 nm as the optimal excitation peak. It is because the three ligands of p-BBA also form a large conjugated structure after coordination with the Tb(III) ions, producing a broad excitation band. The emission spectrum was excited by the wavelength of 280 nm, as shown in
Figure 5b. The complex exhibits obvious characteristic emissions of the Tb(III) ions at 490, 545, 585 and 623 nm, which are attributed to f-f transition of the Tb(III) ions at
5D
4–
7F
6,
5D
4–
7F
5,
5D
4–
7F
4 and
5D
4–
7F
3. The strongest emission peak at 545 nm belongs to the hypersensitive transition [
27], which shows strong sharp-line narrow-band pure green emission. The luminescence process of the complex Tb(p-BBA)
3UA is similar to that of the complex Eu(TTA)
2(phen)UA, meeting the energy transfer requirement and thus exhibiting the characteristic emission of the Tb(III) ions.
3.5. Effect of Relative Molecular Weight on the Luminescent Properties of the Copolymer PMEuTb
The molecular weight and molecular weight distribution of the copolymer PMEuTb with different initiator concentrations were measured by a Waters 410 gel permeation chromatographer with tetrahydrofuran as an eluent, as shown in
Table 2. With the increase of initiator concentration, the polymerization degree of the copolymer PMEuTb decreases and the number average molecular weight
Mn and the weight average molecular weight
Mw decrease. In the free radical polymerization, the higher the initiator concentration is, the more primary free radicals generate in the chain initiation stage and the more monomer free radicals form. However, the amount of the monomer is constant and the number of monomers on the molecular chain decrease, resulting in a decrease in molecular weight. On the other hand, the polymerization degree of the polymer in free radical polymerization is relevant to four facts: normal polymerization, transfer to the monomer, transfer to the initiator and transfer to the solvent. The monomer is methyl methacrylate, and its chain transfer constant to the monomer is small, about 10
−4~10
−5, which can be ignored. The initiator used in the experiment is AIBN. In this work, the chain transfer constant is 0.02, which is relatively small. The solvent in the experiment is dimethyl sulfoxide, there are no active hydrogen atoms or halogen atoms in the molecule and the chain transfer constant is relatively small. No chain transfer agent was added during the polymerization. Therefore, in this free radical polymerization system, the degree of polymerization of the polymer is only relevant to normal polymerization, and the chain termination is dominated by diradical termination. The higher the concentration of free radicals, the higher the probability of double group termination, and the chain termination stage comes earlier, resulting in the decrease of molecular weight. The molecular weight distribution index of the copolymer is 1.5~2.0, demonstrating that the molecular weight distribution is narrow and the molecular weight distribution is relatively uniform.
In order to investigate the effect of different initiator concentrations on the luminescent properties, the excitation wavelength was set at 254 nm, the resolution was set at (5.0, 5.0 nm) and the phosphorescent emission spectra of serial copolymers PMEuTb with different initiator concentrations were recorded at room temperature in solid state, as presented in
Figure 6a. It can be learned that the serial copolymers exhibit characteristic emission at 489, 545, 589, 615 and 650 nm. The emission peaks at 489 and 545 nm are attributed to the characteristic emission of the Tb(III) ions, corresponding to the
5D
4–
7F
6 and
5D
4–
7F
5 transitions of the Tb(III) ions; the emission peak at 650 nm is attributed to the characteristic emission of the Eu(III) ions, corresponding to the
5D
0–
7F
3 transition of the Eu(III) ions. The emission peak at 589 nm has a wider FWHM, which is transformed from sharp line emission in the complex to broad peak emission, in that this peak is the superposition of emission peaks at 591 nm (
5D
0–
7F
1 transition) in the Eu(III) ions and at 585 nm (
5D
4–
7F
4 transition) in the Tb(III) ions. FWHM at 615 nm also significantly increases, which is the result of the superposition of the emission peaks at 613 nm (
5D
0–
7F
2 transition) in the Eu(III) ions and at 623 nm (
5D
4–
7F
3 transition) in the Tb(III) ions. The sharp line emission at 510 nm does not appear in the complexes Eu(TTA)
2(phen)UA and Tb(
p-BBA)
3UA, and it is the frequency-doubling emission at the excitation wavelength of 254 nm.
Comparing the luminescent intensity of the serial copolymers PMEuTb with different initiator concentrations, the general trend is that luminescent intensity decreases with the increase of the initiator concentration. Combined with the molecular weight and distribution of different initiator concentrations, the relative molecular weight of the polymer decreases and the molecular weight distribution gradually increases with the increase of the initiator concentration, indicating that, with the increase of the initiator concentration, the molecular chain gradually is shortened, resulting in more and more dense distributions of complexes in the polymer molecular chain and a non-radiation transition probability increase. Therefore, the luminescent intensity of the serial copolymer PMEuTb decreases with the increase of the initiator concentration. The luminescent intensity of the copolymer with an initiator concentration of 0.1% is the highest. In the subsequent experiments, the copolymer with an initiator concentration of 0.1% is selected for further research.
The phosphorescent emission spectra of the serial copolymer PMEuTb with different initiator concentrations were measured by 365 nm of ultraviolet light at the resolution (5.0, 5.0 nm), as shown in
Figure 6b. The serial copolymers exhibit characteristic emission at 489, 545, 589, 615 and 650 nm. The emission peaks at 489 and 545 nm correspond to the
5D
4–
7F
6 and
5D
4–
7F
5 transitions of the Tb(III) ions and the emission peak at 650 nm is attributed to the
5D
0–
7F
3 transitions of the Eu(III) ions. The FWHM at 589 nm is wider, which is the superposition of emission peaks of the
5D
0–
7F
1 transition of the Eu(III) ions at 591 nm and the
5D
4–
7F
4 transition of the Tb(III) ions at 585 nm. Different from the emission spectra excited at 254 nm, the maximum emission intensity is located at 615 nm, being pure red-light emission.
According to the phosphorescent emission spectra of the series of copolymers, their CIE color coordinates were calculated, as shown in respective subgraphs of
Figure 6. When the excitation wavelength is 254 nm, its color coordinate is located in the green region because the emission intensity of the green complex Tb(
p-BBA)
3UA is 3597, while that of the red complex Eu(TTA)
2(Phen)UA’s emission intensity is only 788. When the excitation wavelength is set as 365 nm, its color coordinate is in the red-light region. Therefore, when 365 nm is used as the excitation wavelength, its luminescence displays mainly red-light emission. These data enable us to conclude that the copolymer PMEuTb has dual-wavelength emission characteristics.
3.6. Luminescent Properties of the Copolymer PMEuTb with Initiator Concentration of 0.1%
The copolymer PMEuTb with an initiator concentration of 0.1% was selected as the research object, the resolution was set as (1.0 nm, 1.0 nm) and the excitation spectra were measured with 615 nm and 545 nm as the monitoring wavelengths, as shown in
Figure 7. The copolymer PMEuTb exhibits a strong excitation band at 220~400 nm, mainly due to the joint action from the complexes Tb(
p-BBA)
3UA and Eu(TTA)
2(phen)UA. The optimal excitation wavelengths of the copolymer PMEuTb are both located at 270 nm under the monitoring of 615 nm and 545 nm wavelengths. Compared with the monomers, the optimal excitation wavelengths are all blue-shifted. In addition, the excitation wavelengths change from 285 nm and 365 nm in the complex Eu(TTA)
2(phen)UA to 270 nm and 365 nm in PMEuTb, and the optimal excitation wavelength changes from 365 nm to 270 nm. It may be because the ligand
p-BBA of Tb(III) ions indirectly excited the Eu(III) ions after the red and green light complex monomers were copolymerized with methyl methacrylate, resulting in the excitation wavelength scope and optimal excitation peak at the monitoring wavelength of 615 nm being consistent with that of 545 nm.
Since 254 nm and 365 nm UV lamps are common on the market, the emission spectrum of the copolymer was measured by using excitation wavelengths of 254 nm and 365 nm, as shown in
Figure 7. As can be seen from the figure, both spectra show characteristic emission peaks at 490, 545, 589, 615 and 654 nm. Among them, the emission peaks at 490 nm and 545 nm are attributed to the characteristic emission of the Tb(III) ions. The peaks at 615 nm and 654 nm correspond to the characteristic emission of the Eu(III) ions. The emission peak at 589 nm has a wider FWHM, which is the result of superposition at the 591 nm of the Eu(III) ions and the 585 nm of the Tb(III) ions. Compared with the complex Eu(TTA)
2(phen)UA, characteristic emission at 613 nm redshifts to 615 nm in the copolymer PMEuTb, still maintaining the characteristic sharp line emission. This is owing to the fact that the
f-
f level transition of
5D
0–
7F
2 is a hypersensitive transition and is easily affected by surroundings, leading to a slight red shift of characteristic emission in the copolymer. The difference is that the luminescent performance of the emission spectrum is different with different excitation wavelengths. Under 254 nm excitation, the green-light emission peak of 545 nm is strong and the red-light emission peak of 615 nm is weak, demonstrating green-light emission in whole. However, under 365 nm excitation, the red-light emission peak of 615 nm is strong and the green-light emission peak is relatively weak, displaying red-light emission in whole, as shown in the color of the luminescent photo in
Figure 7. Therefore, the copolymer is a kind of dual-wavelength bonded luminescent material, which can be used to prepare dual-wavelength anti-counterfeit fibers.
3.7. Variation-Temperature Luminesecent Spectra of the Copolymer PMEuTb
A variable temperature luminescent spectrum is one of the key indicators of thermal quenching performance of luminescent materials. In order to investigate the thermal quenching properties of the copolymer PMEuTb, taking 365 nm as an example, its temperature-variable luminescent spectra were measured in the range of 293~433 K, as shown in
Figure 8a. The copolymer mainly exhibits red-light emission of the Eu(III) ions under the excitation of 365 nm, which is the optimized excitation wavelength of the complex Eu(TTA)
2(phen)UA, resulting that the luminescent intensity in the copolymer at 615 nm is the strongest. The luminescent intensity at 615 nm is the research object, and the plot of the variation of integrated area at 615 nm with temperature is shown in
Figure 8b.
The relative thermal sensitivity (
Sr) is calculated by the following Equation (1) [
28]
where ∆ is the thermometric parameter (in this case, the integrated area of the emission peak at 615 nm) at a certain temperature and
∂∆ is the variation of this signal upon a certain temperature variation (
∂T). The plot of the dependence of relative thermal sensitivity
Sr on
T is presented in
Figure 8b. The figure shows that the emission intensity at 615 nm gradually decreases with the increase of temperature. At 313 K, the luminescent intensity decreases very little and remains at 94% of the initial luminescent intensity and the relative thermal sensitivity
Sr is only 0.31%•K
−1. At 333 K, the luminescent intensity decreases slowly and the copolymer PMEuTb remains at 85% of the initial luminescent intensity with 0.51%•K
−1 of
Sr. The results suggest that the luminescent properties of the copolymer are not affected much by the temperature before 333 K, meet the requirements of room temperature phosphorescent anti-counterfeiting materials [
29]. Starting at 373 K, luminescent intensity acceleratingly declines, which results in only 25% of the initial luminescent intensity at 433 K. The reason for this result is that the copolymer PMEuTb is an amorphous polymer, and the glass transition temperature
Tg of the polymethyl methacrylate is around 378 K [
30]. When the temperature is lower than
Tg, the polymer is in a glass state, the molecular chains and segments keep the static and the monomer units of the red-light and green-light complexes are well fixed in the specific position of the polymer molecular chain. However, the vibration amplitude of atoms (or groups) in the equilibrium position of molecules is aggravated with the increase of temperature, which leads to the decrease of luminescent intensity, but the decrease is not very obvious. However, when the temperature rises above
Tg, the molecular chain segments begin to move, and the polymer is in a highly elastic state. Due to the increased movement of the chain segment, the “cage” effect of the polymer chain segment on the luminescent group is weakened, and the collision probability and non-radiative transition of the luminescent group increase, leading to a sharp decline in luminescent intensity. With the further increase of temperature, the polymer enters the viscous state, the whole molecular chain starts to stretch and move and the luminescent performance of the copolymer is reduced by the influence of the temperature, which displays the decrease of relative thermal sensitivity.
3.8. Luminescent Lifetime of the Copolymer PMEuTb
Using an Edinburgh Instruments FLS980 steady-state/transient fluorescent spectrometer, time-dependent single photon counting (TCSPC) was used to monitor the phosphorescent decay process of the Eu(III) and Tb(III) ions in the luminescent centers of the complex and copolymer. According to Equation (2), double exponential fitting was performed. Then, the average phosphorescent lifetime
τ of the phosphorescent decay curve was calculated according to Equation (3) [
31].
where
τ1 and
τ2 are short and long lifetime, respectively, and
B1 and
B2 are fitting constants.
The excitation wavelength was set as 365 nm, and the phosphorescent decay process of the
5D
0–
7F
2 transition of Eu
3+ in the complex Eu(TTA)
2(phen)UA and the copolymer PMEuTb was monitored, as shown in
Figure 9a,c. The fitting analysis shows that, in the complex,
A = 5.306,
B1 = 18536.23,
B2 = 7688.68,
τ1 = 0.71499 ms,
τ2 = 1.02338 ms and the average lifetime of the complex Eu(TTA)
2(phen)UA calculated by Equation (3) is 0.829 ms. As for the copolymer,
A = 1.346,
B1 = 8336.19,
B2 = 1943.81,
τ1 = 0.38735 ms,
τ2 = 1.08867 ms and the average fluorescence lifetime of the
5D
0–
7F
2 transition of the Eu(III) ions in copolymer PMEuTb was calculated by Equation (3) to be 0.665 ms (the lifetime is between 10
−6 and20 s, which is attributed to the phosphorescent materials). Compared with the complex Eu(TTA)
2(phen)UA, the phosphorescent lifetime decreases from 0.829 ms to 0.665 ms in the copolymer, indicating that the molecular structure of the copolymer has changed. The Eu(III) ions are sensitive to environmental disturbance, and the change of microenvironment leads to the increase of the phosphorescent emission rate constant, so the phosphorescent lifetime of the Eu(III) ions decreases.
The excitation wavelength was set as 254 nm, and the phosphorescent decay process of the
5D
4–
7F
5 transition of the Tb(III) ions in the complex Tb(
p-BBA)
3UA and the copolymer PMEuTb was monitored, as shown in
Figure 9b,d. The fitting analysis shows that, in the complex,
A = 5.878,
B1 = 23109.10,
B2 = 1799.65,
τ1 = 0.8548 ms,
τ2 = 1.8801 ms and the average lifetime of the complex Tb(
p-BBA)
3UA calculated by Equation (3) is 1.005 ms. For the copolymer,
A = 1.164,
B1 = 3682.83,
B2 = 5084.70,
τ1 = 0.6495 ms,
τ2 = 1.2463 ms and the average phosphorescent lifetime of the
5D
4–
7F
5 transition of the Tb(III) ions in the copolymer PMEuTb was calculated by Equation (3) to be 1.083 ms. Compared with the complex Tb(
p-BBA)
3UA, the phosphorescent lifetime of the Tb(III) ions in the copolymer PMEuTb increases, while the phosphorescent lifetime of the Eu(III) ions decreases, which may be caused by the energy transfer from the Eu(III) ions to the Tb(III) ions [
32].