Next Article in Journal
The Effects of High-Grade Metamorphism on Cr-Spinel from the Archean Sittampundi Complex, South India
Next Article in Special Issue
Effect of Sodium Metabisulfite on Selective Flotation of Chalcopyrite and Molybdenite
Previous Article in Journal
Tight Sandstone Reservoir Formation Mechanism of Upper Paleozoic Buried Hills in the Huanghua Depression, Bohai Bay Basin, Eastern China
Previous Article in Special Issue
Effect of Magnesium on the Hydrophobicity of Sphalerite
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Extraction of Potassium from Feldspar by Roasting with CaCl2 Obtained from the Acidic Leaching of Wollastonite-Calcite Ore

Mineral Processing Engineering Department, Faculty of Mines, Istanbul Technical University, Maslak, Istanbul 34469, Turkey
*
Author to whom correspondence should be addressed.
Minerals 2021, 11(12), 1369; https://doi.org/10.3390/min11121369
Submission received: 26 October 2021 / Revised: 29 November 2021 / Accepted: 29 November 2021 / Published: 3 December 2021

Abstract

:
Potassium, which is included in certain contents in the structure of K-feldspar minerals, has a very important function in the growth of plants. Turkey hosts the largest feldspar reserves in the world and is by far the leader in feldspar mining. The production of potassium salts from local natural sources can provide great contributions both socially and economically in the agriculture industry along with glass production, cleaning materials, paint, bleaching powders, and general laboratory purposes. In this study, potassium extraction from K-feldspar ore with an 8.42% K2O content was studied using chloridizing (CaCl2) roasting followed by water leaching. Initially, to produce wollastonite and calcite concentrates, froth flotation tests were conducted on wollastonite-calcite ore after comminution. Thus, wollastonite and calcite concentrates with purities of 99.4% and 91.96% were successfully produced. Then, a calcite concentrate was combined with hydrochloric acid (HCl) under optimal conditions of a 1 mol/L HCl acid concentration, a 60 °C leaching temperature, and a 10 min leaching time to produce CaCl2. To bring out the importance of roasting before the dissolution process, different parameters such as roasting temperature, duration, and feldspar—CaCl2 ratios were tested. Under optimal conditions (a 900 °C roasting temperature, a 60 min duration, and a 1:1.5 feldspar—CaCl2 ratio), 98.6% of the potassium was successfully extracted by the water leaching process described in this article.

1. Introduction

Potassium is an element that occupies an important place in human life and is widely used in different industries as a component of potash. Potassium fertilizer is an essential nutrient, particularly for fruit formation and development. It accelerates plant growth and increases crop yields. In addition to the fertilizer industry, large amounts of potassium salts are used annually to produce glass, cleaning materials, paint, and bleaching powders and for general laboratory purposes [1]. The consumption and cost of potassium salts vary annually and are between 25 and 30 million tons and USD 300 and 500, respectively. In Turkey, potassium salts (potassium chloride (KCl) and potassium sulfate (K2SO4)), which are needed by the chemical and fertilizer industries are provided by imports.
Water-soluble potash is used to produce potassium salts; however, the increase in the need for potassium salts and the decrease in water-soluble potash sources have led the producers to find an alternative source such as K-feldspars. Feldspars constitute more than 60% of the earth’s crust and contain microcline, albite, and aluminum silicate with varying concentrations (5–12%) of potassium oxide (K2O) [2,3,4]. Turkey has approximately 14% of the world’s high-quality feldspar reserves. While the most valuable sodium feldspar deposits are located in Western Anatolia (Çine, Milas, Yatağan, and Bozdoğan regions), the majority of K-feldspar deposits are found in the Kırşehir massive [5,6]. In addition to large K-feldspar reserves, there is also a significant amount of wollastonite-calcite deposits in the Kırşehir–Buzlukdağı region. About 4 million tonnes of potash are imported for agricultural and industrial activities each year in Turkey. KCl and CaCl2 salts, which are the main raw materials of the fertilizer industry, can be obtained from feldspar and wollastonite minerals, respectively. Obtaining these high value-added products from different industrial raw materials in the same geographical region significantly increases resource use and efficiency while reducing costs.
Wollastonite and calcite minerals, which are used in ceramics, plastics, metallurgy, paint, and other industries are usually found in the same deposits. The most common method for separating these two industrial minerals is flotation. As wollastonite has a needle-like structure, the flotation process can be performed in the presence of collectors such as amines or fatty acids. In a study by Kangal et al., the best result was obtained at pH 6 and 1500 g/t K-oleate dosage. Under these conditions, a calcite concentrate assaying 55.89% CaO, 0.35% SiO2, 0.03% Fe2O3, and 42.30% loss on ignition (LOI) was produced. At the same time, a wollastonite concentrate containing 52.71% SiO2, 44.65% CaO, 0.44% Fe2O3, and 0.60% LOI was obtained [7]. Several investigations have been carried out to separate wollastonite from calcite-rich wollastonite ore [8,9,10]. Çinku and co-authors indicated that a marketable wollastonite concentrate could be produced by flotation following magnetic separation from wollastonite ore containing 40% CaO and 48% SiO2. As a result of the flotation tests at pH 9, the optimal flotation conditions were determined as 1000 g/t of collector dosage, 1.7 kg/t of sodium silicate, and 500 g/t of caustic soda. Using oleic acid, a concentrate containing 54.43% SiO2, 41.44% CaO, 0.59% Fe2O3, and 0.97% loss on ignition was obtained. In addition, when oleic acid is used, a concentrate assaying 57.10% SiO2, 40.88% CaO, 0.30% Fe2O3, and 0.13% loss on ignition was produced [9]. In another important study by Ravi et al., a 97% purity wollastonite concentrate was obtained from low-content wollastonite ore through the flotation and magnetic separation methods. In the flotation experiments, a particle size of 100 μm and a sodium oleate concentration of 1 kg/t were found to be optimal, and a wollastonite concentrate (about 95% purity) with 2.64% iron content and 0.4% ignition loss was produced [9]. In the study by Bulut and co-authors, a wollastonite (about 87.9% purity) concentrate containing 0.44% Fe2O3 and 52.71% SiO2 with 0.60% loss on ignition was obtained using 1500 g/t of potassium oleate. In addition, a calcite concentrate containing 99.8% CaCO3 was recovered as a by-product with 85.4% recovery [10].
CaCl2 is an essential component for obtaining potassium salts from feldspar. Although it is not conventional to treat wollastonite with acid to produce CaCl2, acidic digestion of wollastonite can be used as a step in the carbonation pathway for CO2 sequestration. Zhang et al. [11] studied the leaching of wollastonite at various hydrochloric acid (HCl) concentrations and temperatures. It was reported that 81.9% and 96.1% of calcium were dissolved using 1 and 4 mol/L HCl, respectively. By maintaining a 4 mol/L HCl concentration, constant leaching tests were performed at different temperatures (40, 60, 80, and 90 °C) and the calcium dissolutions values were achieved as 91%, 96.9%, 97.1%, and 97.5%, respectively.
In the literature, many studies have been carried out to produce KCl from run-of-the-mine feldspar ore using pure CaCl2 salt. Using K-feldspar ore and pure CaCl2, roasting tests were carried out in a high-temperature furnace at various temperatures for 1 h. After the roasting was completed, the leaching process was performed under the constant conditions of a 10% solid-in-pulp ratio, a temperature of 60 °C, and a 500 rpm mixing speed [12]. As a result, a 98.3% potassium extraction was obtained with the dissolution process after roasting at 850 °C. In another study by Kangal et al. [13], a 90% dissolution efficiency was achieved at a 15% solid-in-pulp ratio and at a 40 °C temperature.
Yuan et al. [14] reported a 91% potassium dissolution (under the leaching condition of 70 °C, 30 min, and a solid–liquid ratio of 1:50) from a 50–75 µm potassium feldspar fraction with a 13.25% K2O content by roasting at 900 °C for 40 min with a 1:1.15 CaCl2–potassium feldspar ratio. Serdengeçti et al. [15] investigated the production of KCl from a potassium feldspar ore containing 9.69% K2O and succeeded in dissolving 99.8% of potassium through water leaching (a 60 °C temperature and a 120 min leaching time) following the roasting process (1:1.5 potassium feldspar—CaCl2 ratio, 850 °C of temperature, and 60 min of roasting time). Samantray et al. [16] investigated the effects of the CaCl2 amount, roasting temperature, leaching time, and temperature on KCl production from feldspar ore containing 11.64% K2O. After roasting at 900 °C and with a ratio of 1:1 CaCl2—feldspar, more than 80% of potassium was dissolved after 30 min. Tanvar and Dhawan [17] investigated the effects of additives, roasting temperature, and time on the recovery of potash from feldspar containing 9.67% K2O. Roasting experiments were carried out at 950 °C for 60 min, and CaCl2 was used as the slag material. At the end of citric acid leaching at room temperature, a 1:10 solid–liquid ratio, and 60 min, a 95% potassium dissolution efficiency was achieved. Samantray et al. [18] investigated the extraction of potassium from feldspar ore containing 11.64% K2O using eggshell powder as a calcium source. Feldspar and eggshells were ground together below 45 µm and roasted at 900 °C for 30 min with a 1:1.8 eggshell—feldspar ratio. Then, this mixture was leached with HCl for 30 min at room temperature and a 99% potassium recovery was obtained.
Today, the main approach of beneficiation and production is based on a circular economy and environment. In this study, potassium recovery from K-feldspar ore was achieved using CaCl2 produced from wollastonite-calcite ore in the same region. In the first part of this study, wollastonite-calcite ore was subjected to flotation tests to produce wollastonite and calcite concentrates. High-grade CaCl2 was produced through a HCl acid treatment using a calcite concentrate obtained as a result of flotation. Second, roasting followed by the water leaching process was applied to K-feldspar with CaCl2. With this original and innovative work, the extraction of potassium using wollastonite—calcite and K-feldspar ores located in a similar mineralization zone will be possible, and these local natural resources can be brought into the economy.

2. Materials and Methods

2.1. Material and Characterization

The wollastonite-calcite and potassium feldspar ores were obtained from the Buzlukdagi Region, Kırşehir, Turkey. The representative ore samples were crushed below 2 mm using jaw, cone, and roller crushers, and wet sieving was performed to determine the particle size distribution. According to the results, the d80 size of wollastonite and feldspar samples were found to be 1.2 and 0.5 mm, respectively. The BSE (Back-Scattered Electron) images of samples are given in Figure 1. The chemical contents of the samples (Table 1) were determined by inductively coupled plasma (ICP) at Activation Laboratories Ltd., Hamilton, ON, Canada. To determine the loss on ignition of the samples, the samples were placed in crucibles and weighed. After, they were kept in an oven at 100 °C overnight to remove moisture. Then, the temperature was raised to 550 °C, and the organic materials were completely removed after 4 h. The carbonate structure turned into oxides at 1000 °C after 2 h, and the ratio of the initial and final weight difference to the feed represented the ignition loss.
An X-ray diffraction (XRD) analysis was conducted with a copper X-ray-sourced Panalytical X’Pert Pro diffractometer (Malvern Panalytical Ltd., Malvern, UK). PDF-4/Minerals International Centre of Diffraction Data (ICDD) software (PDF-4/Minerals, ICDD, Delaware County, PA, USA) was used for mineral characterization. The crystals’ mineral phase ratio was determined through the Rietveld method. XRD patterns of wollastonite-calcite and feldspar samples are shown in Figure 2 and Figure 3, respectively. According to the results, the secondary mineral was calcite in the wollastonite-calcite sample and the feldspar sample mostly consisted of potassium feldspar.
The chemical and mineralogical properties of samples were defined with a differential thermal analysis (DTA) and the thermogravimetric analysis (TGA) equipment’s STA 449 F3 Jupiter® thermal analyzer (NETZSCH, Selb, Germany). DTA and TGA curves of wollastonite-calcite, calcite concentrate (from flotation), and feldspar samples are illustrated in Figure 4, Figure 5 and Figure 6, respectively.
As can be seen in Figure 4, a loss of 21% of weight occurs in the wollastonite ore as the temperature rises from 700 °C to 950 °C. The main reason for this loss is calcite, which constitutes more than 50% of the structure of the ore. The DTA and TGA results shown in Figure 5 indicate that a significant amount of structural deterioration occurred at 900 °C. Only 0.6% of weight loss was determined in the feldspar ore sample between 400 and 800 °C (Figure 6). Partial structural deterioration was encountered at 700–750 °C. This small loss might be explained by probable carbonate components in the ore.

2.2. Methods

Calcite must be treated with hydrochloric acid to produce CaCl2. Calcite reacts with HCl to form CaCl2 and releases CO2 and H2O as by-products (Equation (1)) [19].
CaCO3 + 2HCl → CaCl2 + CO2 + H2O
The potassium dissolution process can be finished by mixing the CaCl2 obtained in the first equation with K-feldspar ore in certain proportions and by subjecting them to roasting and leaching processes. The mixture of feldspar and CaCl2, which is exposed to a temperature higher than the decomposition temperature during the roasting process, reacts to form KCl salt. On the other hand, quartz and anorthite minerals are produced as by-products (Equation (2)) [14].
Since the KCl salt obtained as a result of this process is easily soluble, it can be taken into a solution by leaching with water.
CaCl2 + 2KAlSi3O8 → CaAl2Si2O8 + 4SiO2 + 2KCl
In the first step, wollastonite-calcite ore was subjected to comminution (below 75 μm) and then froth flotation was used to separate calcite and wollastonite. An amount of 300 gr of wollastonite-calcite ore was subjected to self-aerated Denver flotation equipment with a 1.5 L cell volume and a 1200 rpm mixing rate. The conditions of the flotation tests are given in Table 2. While calcite particles were floated with the help of a collector, wollastonite particles were not activated and taken as the sinking product. Afterward, the calcite concentrate was subjected to HCl acid leaching (Figure 7). Different HCl concentrations (0.25, 0.5, 2, 3, 4, and 6 mol/L), temperatures (25, 40, 60, and 80 °C), and leaching times (5, 10, 15, 30, 60, 90, and 120 min) were investigated to determine the optimal treatment conditions with a constant 1:2 solid–liquid ratio. After obtaining the pregnant solution, CaCl2 was precipitated by evaporation. Second, the CaCl2 sample obtained from the calcite concentrate was ground and mixed in an agate mortar with potassium feldspar in a 1:1.5 feldspar–CaCl2 ratio until it had a homogeneous appearance. Afterward, 7.5 g of the mixture was spread in a thin layer on four porcelain crucibles (diameter: 8 cm) and the roasting tests were performed in a Protherm brand PLF 130/6 furnace at elevated temperatures of 800, 850, 900, and 950 °C for 1 h. After roasting, water leaching was performed for 2 h under constant conditions, namely a 10% solid-in-pulp ratio, a 60 °C temperature, and a 500 rpm mixing speed.
After acid leaching, titration was used to determine HCl consumption. A 0.01 mol/L NaOH solution was prepared and transferred into a 10 mL burette. A beaker containing 30 mL of the test solution was placed under the burette. Four drops of phenolphthalein (a color-change indicator) were added to the solution, and the burette faucet was opened enough to allow a single droplet to pass. A 0.01 mol/L NaOH solution was mixed into the solution until it turned pink, at which point the faucet was closed, and the spent NaOH was detected. Lab-scale vacuum equipment with fine filter paper (Sartorius brand 391 code, blue label) was used for liquid–solid separation and the filtered cake was dried at 70 °C for approximately 24 h. The elemental analysis of the liquid was provided by the atomic absorption spectrometer (Varian brand AA240FS, Palo Alto, CA, USA).

3. Results and Discussion

3.1. Flotation of Wollastonite-Calcite Ore

To produce CaCl2 for the roasting and leaching experiments, previously, wollastonite-calcite ore was subjected to flotation experiments after comminution, and a calcite concentrate with low iron content was obtained in the first two flotation stages. In the following steps, the augite mineral was activated and started to float. On the other hand, wollastonite was not activated and remained in the cell despite the increasing potassium oleate concentration. As seen in Table 3, Float-1 and Float-2 products contained high grades of CaCO3, 91.55% and 92.77%, respectively. Float-3, Float-4, and Float-5 were characterized as tailings, since their Fe2O3 contents were high. A marketable wollastonite concentrate having a 99.4% purity was produced with 0.44% Fe2O3, 0.95% CaCO3, and 49.70% SiO2 contents using a 1500 g/t potassium oleate. Calcite concentrates obtained in the first two flotation stages were combined and a final calcite concentrate (91.96% CaCO3) with 0.11% Fe2O3 and 2.14% SiO2 was produced.

3.2. CaCl2 Production by Acid Leaching

The final calcite concentrate obtained after the flotation process was treated with HCl to produce CaCl2. The effects of the concentration, temperature, and time on acid leaching were investigated. After the determination of the most suitable condition, CaCl2 was mixed with potassium feldspar in certain proportions, the roasting and dissolution processes were completed, and finally, potassium was successfully extracted.

3.2.1. Effect of HCl Concentration

Based on the formula in Equation (1), the acid treatment was applied to the calcite concentrate. HCl was used as a solvent to investigate the effect of various acid concentrations (0.25, 0.5, 1, 2, 3, 4, and 6 mol/L) on CaCl2 production. The leaching temperature and time were chosen as 60 °C and 10 min, respectively. The HCl-Calcite ratio was adjusted to 2:1 by weight. Calcium dissolution efficiencies versus acid concentration are illustrated in Figure 8.
Figure 8 clearly shows that 2 mol/L HCl provides an optimal calcium extraction rate of 93.7%. The 2 mol/L HCl concentration was kept constant in the following experiments, as there was no more than a 3% increase in dissolution efficiency at higher acid concentrations. Similar results were obtained in the study of Zhang et al. [11], who performed the dissolution experiments to produce CaCl2. The highest calcium dissolution rate (96.1%) was obtained at a 4 mol/L HCl concentration, while 1 mol/L HCl led to only 81.9% calcium dissolution. To determine the amount of HCl consumption for our case, the titration method was chosen and the acid consumption was found to be 165 kg/ton for this study.

3.2.2. Effect of Temperature

After a suitable acid concentration was obtained, the effect of temperature on calcium dissolution efficiency was investigated at different temperatures (25, 40, 60, and 80 °C). The HCl–Calcite ratio was kept constant at 2:1, and tests were performed with a 10 min leaching time, a mixing speed of 350 rpm, and 2 different HCl concentrations (1 and 2 mol/L). The calcium dissolution efficiencies are presented in Figure 9.
The results in Figure 9 indicated that the leaching temperature had a considerable effect on the dissolution of calcium. Especially, no significant change was observed after the 2 mol/L HCl concentration at 40 °C. On the other hand, calcium dissolution yields increased continuously with increasing temperature while the dissolution of calcium started to stabilized after the 1 mol/L HCl concentration at 60 °C. Considering the gelation problem caused by the use of a vacuum after the experiment using a 2 mol/L HCl concentration, a 1 mol/L HCl concentration, and a 60 °C temperature were found to be more suitable for the dissolution process. Zhang et al. [11] indicated the importance of temperature on leaching in their study. After 20 min of dissolution at a 4 mol/L HCl concentration, 91.0%, 96.9%, 97.1%, and 97.5% calcium dissolution efficiencies were achieved at 40, 60, 80, and 90 °C, respectively.

3.2.3. Effect of Leaching Time

The effect of leaching time on the calcium dissolution was investigated using various durations (5, 10, 15, 30, 60, 90, and 120 min). The HCl-Calcite ratio was kept constant at 2:1, and tests were performed at a 1 mol/L HCl concentration, a 60 °C temperature, and a mixing speed of 350 rpm. The results are shown in Figure 10. As seen in Figure 10, although there is not much change in recovery, the recovery decreases as the leaching time increases. A 5 min leaching time is not considered sufficient for the system to balance; therefore, a 10 min leaching time was preferred.

3.3. The Roasting Followed by Leaching

Roasting followed by water leaching was investigated by adopting Equation (2). CaCl2 produced in the previous process was treated with K-feldspar. The aim was to replace calcium ions with potassium at temperatures above the melting point of the feldspar sample. The feldspar—CaCl2 ratio was kept constant at 1:1.5, and the mixture was roasted at different roasting temperatures (800, 850, 900, and 950 °C) for an hour. Water was used as a solvent to dissolve the potassium from the roasted sample. Under constant conditions, a pregnant solution containing potassium ions was obtained. Table 4 shows the results of the roasting process followed by leaching.
According to the results, the highest potassium extraction was achieved at a 900 °C roasting time. Since CaCl2 is an expensive additive, producing CaCl2 from local reserves can be helpful in improving both the usage of natural resources and in producing high-value-added products. In light of the data obtained in this study, it is possible to design a process that allows for the recovery of potassium from wollastonite-calcite and K-feldspar ores in the same region.

4. Conclusions

As it is known, mineral processing is very significant in terms of both technological and economic evaluation of raw materials before chemical beneficiation. In this study, using K-feldspar and CaCl2 roasting followed by leaching tests were performed to extract potassium from the natural resources that were located in the same district. For that purpose, the comminuted wollastonite-calcite ore was subjected to flotation tests, and a marketable wollastonite concentrate and a high purity CaCO3 were produced. Calcite concentrate from the flotation test was treated with HCl to produce CaCl2. Under the optimal conditions of a 1 mol/L HCl acid concentration, a 60 °C leaching temperature, and a 10 min leaching time, 92.7% of calcium was extracted. The CaCl2 produced by the evaporation method was mixed with K-feldspar in certain proportions and then subjected to roasting experiments followed by dissolving experiments. The optimal feldspar–CaCl2 ratio was found to be 1:1.5, and 98.6% of the potassium was successfully extracted from the potassium feldspar ore. It is inevitable for economic development to produce KCl, which is very important for the fertilizer industry, from wollastonite-calcite and K-feldspar ores in the same region. Obtaining high-value-added products from different industrial raw materials increases the added value of the raw material considerably and will enable Turkey to use its natural resources more efficiently.

Author Contributions

T.T., Z.Ü., F.B., G.B. and M.O.K. conceived and designed the experiments; T.T., Z.Ü. and M.O.K. performed the experiments and analyzed the data; T.T., Z.Ü., F.B., G.B. and M.O.K. contributed to writing the paper. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Istanbul Technical University Circulating Capital Enterprise R&D, Project ID: 42017.

Data Availability Statement

No applicable.

Acknowledgments

The authors express their sincere thanks and appreciation to Istanbul Technical University Circulating Capital Enterprise R&D and BS Invest Co. for financial support and for kindly providing the feldspar samples.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Scherer, H.W.; Mengel, K.; Dittmar, H.; Drach, M.; Vosskamp, R.; Trenkel, M.E.; Gutser, R.; Steffens, G.; Czikkely, V.; Niedermaier, T.; et al. Fertilizers. In Ullmann’s Encyclopedia of Industrial Chemistry; Wiley-VCH Verlag GmbH & Co. KGaA: Weinheim, Germany, 2002. [Google Scholar]
  2. Burat, F.; Kökkiliç., O.; Kangal, O.; Gürkan, V.; Çelik, M.S. Quartz-feldspar separation for glass and ceramic industry. Miner. Metall. Process. 2007, 24, 75–80. [Google Scholar] [CrossRef]
  3. Kalyoncu, E.; Burat, F. Selective separation of coloring ımpurities from feldspar ore by ınnovative single-stage flotation. Miner. Process. Extr. Metall. Rev. 2021, 42, 1–6. [Google Scholar] [CrossRef]
  4. Rao, J.R.; Nayak, R.; Suryanarayana, A. Feldspar for potassium, fertilisers, catalysts and cement. Asian J. Chem. 1998, 10, 690–706. [Google Scholar]
  5. Kangal, M.O.; Bulut, G.; Yeşilyurt, Z.; Güven, O.; Burat, F. An alternative source for ceramics and glass augen-gneiss. Minerals 2017, 7, 70. [Google Scholar] [CrossRef] [Green Version]
  6. Kangal, M.O.; Bulut, G.; Yeşilyurt, Z.; Baştürkcü, H.; Burat, F. Characterization and production of Turkish nepheline syenites for industrial applications. Physicochem. Probl. Miner. Process. 2019, 55, 605–616. [Google Scholar]
  7. Kangal, M.O.; Bulut, G.; Guven, O. Physicochemical characterization of natural wollastonite and calcite. Minerals 2020, 10, 228. [Google Scholar] [CrossRef] [Green Version]
  8. Çinku, K.; Ipekoğlu, B.; Tulgarlar, A. Enrichment of Karaköy wollastonite ore. Ind. Miner. Symp. 1997, 86–91. [Google Scholar]
  9. Ravi, B.P.; Krishna, S.J.G.; Patil, M.R.; Kumar, P.S.; Rudrappa, C.; Naganoor, P.C. Beneficiation of a wollastonite from Sirohi, Rajasthan. Int. J. Innov. Sci. Eng. Technol. 2014, 1, 450–453. [Google Scholar]
  10. Bulut, G.; Akçin, E.S.; Kangal, M.O. Value added industrial minerals production from calcite-rich wollastonite. Gospod. Surowcami Miner. 2019, 35, 43–58. [Google Scholar]
  11. Zhang, J.; Zhang, R.; Geerlings, H.; Bi, J. A novel indirect wollastonite carbonation route for CO2 sequestration. Chem. Eng. Technol. 2010, 33, 1177–1183. [Google Scholar] [CrossRef]
  12. Kangal, M.O.; Bulut, G.; Burat, F.; Üçerler, Z.; Türk, T. Developing a Process for Obtaining High Value Added KCl with Calcium Chloride to be Produced from Kirşehir High Calcite Content Wollastonite; R&D Project, Final Report; ITU, Mineral Processing Engineering Department: İstanbul, Turkey, 2019; 39p. (In Turkish) [Google Scholar]
  13. Kangal, M.O.; Burat, F.; Güney, A.; Türk, T.; Şavran, C. Development of Processes for Obtaining High Value Added Potassium Salts from Turkish Potassium Feldspar Ore; Final Report; The Scientific and Technological Research Council of Turkey (Project No: 218M107): İstanbul, Turkey, 2019; 53p. (In Turkish) [Google Scholar]
  14. Yuan, B.; Li, C.; Liang, B.; Lü, L.; Yue, H.; Sheng, H.; Xie, H. Extraction of potassium from K-feldspar via the CaCl2 calcination route. Chin. J. Chem. Eng. 2015, 23, 1557–1564. [Google Scholar] [CrossRef]
  15. Serdengeçti, M.T.; Baştürkcü, H.; Burat, F.; Kangal, M.O. The correlation of roasting conditions in selective potassium extraction from K-feldspar ore. Minerals 2019, 9, 109. [Google Scholar] [CrossRef] [Green Version]
  16. Samantray, J.; Anand, A.; Dash, B.; Ghosh, M.K.; Behera, A.K. Sustainable process for the extraction of potassium from feldspar using eggshell powder. ACS Omega 2020, 5, 14990–14998. [Google Scholar] [CrossRef] [PubMed]
  17. Tanvar, H.; Dhawan, N. Recovery of potash values from feldspar. Sep. Sci. Technol. 2020, 55, 1398–1406. [Google Scholar] [CrossRef]
  18. Samantray, J.; Anand, A.; Dash, B.; Ghosh, M.K.; Behera, A.K. Production of potassium chloride from K-feldspar through roast–leach–solvent extraction route. Trans. Indian Inst. Met. 2019, 72, 2613–2622. [Google Scholar] [CrossRef]
  19. Lund, K.; Fogler, H.S.; McCune, C.C.; Ault, J.W. Acidization-II. The dissolution of calcite in hydrochloric acid. Chem. Eng. Sci. 1975, 30, 825–835. [Google Scholar] [CrossRef] [Green Version]
Figure 1. BSE images of wollastonite-calcite and feldspar samples.
Figure 1. BSE images of wollastonite-calcite and feldspar samples.
Minerals 11 01369 g001
Figure 2. X-ray diffraction patterns of the wollastonite-calcite sample.
Figure 2. X-ray diffraction patterns of the wollastonite-calcite sample.
Minerals 11 01369 g002
Figure 3. X-ray diffraction patterns of the potassium feldspar sample.
Figure 3. X-ray diffraction patterns of the potassium feldspar sample.
Minerals 11 01369 g003
Figure 4. DTA-TGA curves of the wollastonite-calcite sample.
Figure 4. DTA-TGA curves of the wollastonite-calcite sample.
Minerals 11 01369 g004
Figure 5. DTA–TGA curves of the calcite concentrate.
Figure 5. DTA–TGA curves of the calcite concentrate.
Minerals 11 01369 g005
Figure 6. DTA–TGA curves of the potassium feldspar sample.
Figure 6. DTA–TGA curves of the potassium feldspar sample.
Minerals 11 01369 g006
Figure 7. General flowchart of the chemical processing following flotation.
Figure 7. General flowchart of the chemical processing following flotation.
Minerals 11 01369 g007
Figure 8. Calcium dissolution curve as a function of acid concentration.
Figure 8. Calcium dissolution curve as a function of acid concentration.
Minerals 11 01369 g008
Figure 9. Calcium dissolution efficiency curve in different hydrochloric acid concentrations depending on temperature.
Figure 9. Calcium dissolution efficiency curve in different hydrochloric acid concentrations depending on temperature.
Minerals 11 01369 g009
Figure 10. Calcium dissolution curve at different leaching times.
Figure 10. Calcium dissolution curve at different leaching times.
Minerals 11 01369 g010
Table 1. Chemical analyses of the representative samples.
Table 1. Chemical analyses of the representative samples.
CompoundContent, %
Wollastonite-CalciteK-Feldspar
SiO228.0062.30
Al2O31.9118.70
Fe2O30.451.89
TiO20.040.20
Na2O0.474.32
K2O0.408.40
CaO48.202.16
MgO1.150.26
P2O50.030.09
SrO0.040.14
MnO0.030.06
LOI20.801.83
LOI: Loss on ignition.
Table 2. The conditions of the flotation experiment.
Table 2. The conditions of the flotation experiment.
Particle Size−74 µm
pH6.0
KOl Dosage300 + 300 + 300 + 300 + 300 g/t
Conditioning Time10 + 5 + 5 + 5 + 5 min
Flotation Time2 + 2 + 1 + 1 + 1 min
Table 3. Results of flotation tests.
Table 3. Results of flotation tests.
ProductsWeight (%)Fe2O3SiO2Loss on IgnitionCalciteWollastonite
CDCDCDPDPD
Float-1 *31.10.096.21.551.840.2859.391.5559.33.101.8
Float-2 *15.80.155.33.302.040.8230.692.7730.66.602.0
Float-32.91.318.524.202.736.475.182.895.148.402.7
Float-43.32.1716.040.805.217.522.839.822.881.605.2
Float-53.13.0921.445.605.48.831.320.071.391.205.4
Sink43.80.4442.649.7082.90.420.90.950.999.4082.9
Total100.00.45100.026.24100.021.08100.047.90100.052.47100.0
C: Content; D: Distribution; P: Purity. * Combined flotation products.
Table 4. Potassium dissolution recoveries after roasting with calcium chloride.
Table 4. Potassium dissolution recoveries after roasting with calcium chloride.
Roasting Temperature, °CPotassium Recovery, %
80097.1
85097.1
90098.6
95097.3
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Türk, T.; Üçerler, Z.; Burat, F.; Bulut, G.; Kangal, M.O. Extraction of Potassium from Feldspar by Roasting with CaCl2 Obtained from the Acidic Leaching of Wollastonite-Calcite Ore. Minerals 2021, 11, 1369. https://doi.org/10.3390/min11121369

AMA Style

Türk T, Üçerler Z, Burat F, Bulut G, Kangal MO. Extraction of Potassium from Feldspar by Roasting with CaCl2 Obtained from the Acidic Leaching of Wollastonite-Calcite Ore. Minerals. 2021; 11(12):1369. https://doi.org/10.3390/min11121369

Chicago/Turabian Style

Türk, Tülay, Zeynep Üçerler, Fırat Burat, Gülay Bulut, and Murat Olgaç Kangal. 2021. "Extraction of Potassium from Feldspar by Roasting with CaCl2 Obtained from the Acidic Leaching of Wollastonite-Calcite Ore" Minerals 11, no. 12: 1369. https://doi.org/10.3390/min11121369

APA Style

Türk, T., Üçerler, Z., Burat, F., Bulut, G., & Kangal, M. O. (2021). Extraction of Potassium from Feldspar by Roasting with CaCl2 Obtained from the Acidic Leaching of Wollastonite-Calcite Ore. Minerals, 11(12), 1369. https://doi.org/10.3390/min11121369

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.