Next Article in Journal
PCL/Gelatin/Graphene Oxide Electrospun Nanofibers: Effect of Surface Functionalization on In Vitro and Antibacterial Response
Next Article in Special Issue
Transverse Magnetic Surface Plasmons in Graphene Nanoribbon Qubits: The Influence of a VO2 Substrate
Previous Article in Journal
Cost-Effective and Facile Fabrication of a Tattoo Paper-Based SERS Substrate and Its Application in Pesticide Sensing on Fruit Surfaces
Previous Article in Special Issue
Totally Spin-Polarized Currents in an Interferometer with Spin–Orbit Coupling and the Absence of Magnetic Field Effects
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Controllable Connection of Fe2Se3 Double Chains and Fe(dien)2 Complexes for Organic–Inorganic Hybrid Ferrimagnet with a Large Coercivity

1
Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, 72 Wenhua Road, Shenyang 110016, China
2
School of Materials Science and Engineering, University of Science and Technology of China, 72 Wenhua Road, Shenyang 110016, China
3
Instrumental Analysis and Research Center, Dalian University of Technology, Panjin 124221, China
*
Author to whom correspondence should be addressed.
Nanomaterials 2023, 13(3), 487; https://doi.org/10.3390/nano13030487
Submission received: 25 December 2022 / Revised: 16 January 2023 / Accepted: 23 January 2023 / Published: 25 January 2023

Abstract

:
Organic–inorganic hybrid materials built by inorganic and organic building units have attracted intensive interest in the past decades due to unique chemical and physical properties. However, rare organic–inorganic hybrid materials show excellent permanent magnetic properties. Here, we develop a facile chemical solution method to bottom-up synthesize a new hybrid (Fe2Se3)2[Fe(dien)2]0.9. This hybrid phase with the space group P21/c (14) possesses a rodlike shape with a diameter of 100–2000 nm and a length of 5–50 µm. The hybrid rods are ferrimagnetic with a Curie temperature (TC) of 11 K. They show a high coercivity (HC) of 4.67 kOe and a saturation magnetization (MS) of 13.5 emu/g at 2 K. Compared with orthorhombic (FeSe2)2Fe(dien)2, the excellent magnetic performance of the hybrid rods is ascribed to the monoclinic hybrid structure built by Fe(dien)2 complexes and Fe2Se3 double chains. Our study provides guidance for connecting inorganic fragments of FeSe2 single chains, Fe2Se3 double chains or β-Fe3Se4 layers with Fe(dien)2 complexes for organic–inorganic hybrid phases with varied crystal structures and magnetic properties.

1. Introduction

Over the past years, the development of organic magnetic materials has been intensively explored for both fundamental research and technological applications [1]. Organic–inorganic hybrid materials combining both organic and inorganic components exhibit diverse structures and unique physical and chemical properties. The advantages of organic–inorganic hybrid materials have attracted strong interest in potential applications in electronic and optical devices [2,3], protective coatings [4], catalysts [5], high-temperature superconductors [6], and so on. Many organic–inorganic hybrid materials are antiferromagnetic or weak ferromagnetic (ferrimagnetic) with low magnetic ordering temperatures [7,8,9,10,11]. Separation of magnetic inorganic fragments, such as one-dimensional (1D) chains [12,13] and 2D plates [14], by organic molecules or complexes results in the magnetism of organic–inorganic hybrid materials, and their magnetic ordering temperatures are usually much below room temperature [15,16,17,18]. Nevertheless, there are rare magnetic organic–inorganic hybrid materials, for example, (Fe2Se3)4[Fe(tepa)] (tepa = tetraethylenepentamine) [19], (β-Fe3Se4)4[Fe(teta)1.5] (teta = triethylenetetramine) [20] and (NH3–CH2–C6H4CO2H)[SnCl6] [21], showing their magnetic ordering temperatures higher than room temperature. Moreover, Fe3+ vacancy doping gives rise to a room-temperature long-range ferrimagnetic (FIM) order in an organic–inorganic hybrid (FeSe2)2Fe(dien)2 (dien = diethylenetriamine) [22]. Noncompensated spins in the (Fe0.86Se2)2Fe(dien)2 due to Fe3+ vacancies are produced by controllable self-assemble of 1D FeSe2 short chains and Fe(dien)2 complexes [22], which is different from the “chemical scissors” model to bond isolated single FeSe2 chains with Fe(dien)2 complexes [13,17]. Moreover, most organic–inorganic hybrid materials have low coercivities. It is very difficult to improve coercivity for organic and inorganic hybrid materials. It is preferable to control the stoichiometry of the inorganic component and the combination of inorganic and organic fragments for excellent magnetic performance. From the point of view of magnetism, it is necessary to develop a “bottom-up self-assemble” that is able to enhance the magnetic properties of organic–inorganic hybrid materials through tuning magnetic interactions between Fe-amine complexes and FexSe building blocks in different dimensions [23]. In comparison with a “top-down” method to synthesize organic–inorganic hybrid materials [24], the “bottom-up self-assemble” is more conducive to manipulating the assemble process at the atomic/molecular level. Recently, quasi-1D spin-ladder compounds, MFe2Se3 (M = Ba, Cs), have attracted considerable interest [25,26,27,28], in which iron and selenium form Fe2Se3 double chains. FeSe4 tetrahedra sharing edges in Fe2Se3 double chains are much different from the FeSe2 single chains mentioned above. More recently, we reported a new type of iron chalcogenide-based superconducting system, which originates from a suppression of the long-range FIM order of a parent phase, [Fe(tepa)](β-Fe2Se3)4, through simultaneously tuning the host and the spacer layers [29].
In this work, we report a facile solution-based synthetic route to fabricate a new organic–inorganic hybrid magnet built by organic Fe(dien)2 and inorganic Fe2Se3 double chains. The (Fe2Se3)2[Fe(dien)2]0.9 hybrid forms with a rodlike shape, which is a single phase in a monoclinic crystal structure with the space group P21/c (14). Temperature dependence of magnetization reveals the ferrimagnetism of the (Fe2Se3)2[Fe(dien)2]0.9 rods with the Curie temperature (TC) of 11 K. The coercivity (HC) and saturation magnetization (MS) of the (Fe2Se3)2[Fe(dien)2]0.9 magnet is 4.67 kOe and 13.5 emu/g, respectively, at 2 K. Our study not only provides guidance for developing a chemical solution method for controllable fabrication of a new type of organic–inorganic hybrid materials but also extends a potential application as an organic permanent magnet due to high coercivity of this organic–inorganic hybrid magnet.

2. Materials and Methods

2.1. Chemicals

Iron(III) acetylacetonate [Fe(acac)3, 98%] was purchased from Aladdin reagent company (Shanghai, China). Diethylenetriamine (dien, 99%), acetone (99.7%), and isopropyl alcohol (99.7%) were purchased from Sinopharm Chemical Reagent Co., Ltd. (Shenyang, China). Se powder (99.99%) was purchased from Macklin Biochemical Co., Ltd. (Shanghai, China). All chemicals were used without further purification.

2.2. Synthesis of Monoclinic (Fe2Se3)2[Fe(dien)2]0.9 Nanorods

In a typical synthesis of (Fe2Se3)2[Fe(dien)2] hybrid nanorods, 3.25 mmol Fe(acac)3, 4 mmol Se powder and 40 mL dien were mixed into a 100 mL quartz crucible in a stainless- steel autoclave under magnetic stirring throughout the entire reaction process. Under an argon gas flow, the mixture was kept at room temperature for 1 h, and then was heated to 393 K and kept at this temperature for 1 h to remove moisture and oxygen. Then the temperature was raised to 433 K and kept for 3 h in order that all raw materials were dissolved into the solution. The solution was subsequently heated to 503 K at a rate of 0.4 K·min−1 and maintained for 3 days. At room temperature, the product was centrifuged at 8000 rpm for 5 min. A ThermoFisher inductively coupled plasma (ICP) spectroscopy gave a concentration of 0.0072 and 0.06 mg mL−1, respectively, for Fe and Se ions left in the light-yellow transparent supernatant above the precipitate, suggesting that all the Fe and Se atoms in the starting materials were combined in the hybrid product. The precipitate was washed by 20 mL acetone and 5 mL isopropyl alcohol the first time and then rewashed in 20 mL acetone four times. The product was dried in a vacuum for further characterization.
For comparison, Fe3Se4(dien)2 particles and (Fe3.5Se4)-dien plates were synthesized in a manner similar to the synthesis of monoclinic (Fe2Se3)2[Fe(dien)2]0.9 rods except that the reaction temperature was set to 473 K and 513 K, respectively. The Fe:Se stoichiometry for different hybrid material was determined by the amounts of the Fe and Se precursors. However, a formula of the hybrid plates cannot be determined due to the hybrid phase being mixed with some decomposed tetragonal FexSe.

2.3. Characterization

Powder X-ray diffraction (XRD) was performed on a Rigaku D/Max-2400 diffractometer (Rigaku Inc., Tokyo, Japan) with a Cu Kα radiation source (λ = 0.154056 nm). The software Fullprof was used to refine the structure of the hybrid product. The size, morphology and microstructure of the as-synthesized products were observed by a JSM 6301F field-emission scanning electronic microscope (SEM) (JEOL Inc., Japan) and a Tecnai G2 F20 transmission electronic microscope (TEM) (FEI Inc., Hillsboro, OR, USA) at 200 kV. The elemental compositions of products were determined by Oxford X-ray energy dispersive (EDX) spectroscopy and inductively coupling plasma spectrometry (ICP). Fourier transform infrared (FTIR) spectrum was recorded on a Nicolet iN10 MX & iS10 spectrometer using the KBr pellet technique (Thermo Fisher Inc., Waltham, MA, USA). Thermal gravimetric analysis (TGA) was performed on an STA6000 thermal analyzer (PerkinElmer Inc., Waltham, MA, USA) under N2 flow with a heating rate of 10 K·min−1 between 300 and 800 K. Fe L-edge X-ray absorption spectroscopy (XAS) measurements were performed at Beamline 08U1A of the Shanghai Synchrotron Radiation Facility (SSRF) in total electron yield (TEY) mode at room temperature. Magnetic hysteresis loops and temperature-dependent magnetization in the field-cooling (FC) mode (at H = 100 Oe) were carried out using a superconducting quantum interference device (SQUID) (Quantum Design Inc., San Diego, CA, USA).

3. Results

3.1. Structural Properties

SEM (Figure 1a,b) and TEM (Figure 1d) images illustrate that the hybrid product synthesized at 503 K for 3 days possesses a rodlike shape with a size distribution of about 100–2000 nm for diameter and 5–50 µm for length. The microstructure at the edge of a rod with a large diameter reveals cleavage grooves (Figure 1b), suggesting that the hybrid nanorods with smaller diameters are cleaved down from the rods with large diameters. The selected area electron diffraction (SAED) pattern of a hybrid nanorod in the inset of Figure 1d reveals periodic crystal structure along the longitudinal direction. Compared with the previous iron vacancy doped hybrids [22], clear diffraction points in the SAED pattern show a single crystal feature of the hybrid nanorod, possibly due to the absence of iron vacancies in the hybrid rods. This was supported by the composition analyses. The EDX spectrum as shown in the inset of Figure 1c indicates the presence of Fe, Se, C and N elements, and Fe and Se are the only heavy elements in the hybrid rods. Elemental mapping of a single nanorod (Figure 1e) shows the even distribution of Fe, Se, C, and N in the hybrid rod (Figure 1f–i). The relative molar ratio of Fe to Se in the hybrid rods was determined to be 44.84/55.16 (3.25/4) by EDX, very similar to the value of 3.27/4 determined by the ICP technique. The FTIR spectrum (Figure 2) presents characteristic peaks of dien featured by the vibration bands of –CH2–, –NH2, and –NH. It reveals the incorporation of organic dien molecules in the hybrid structure. Similar to the previous iron vacancy doped hybrids [22], the bands of –NH2 shift from 3360 cm−1 for the asymmetric stretching vibration of free dien molecules to 3289 cm−1 for that of the hybrid rods and from 3280 cm−1 for the symmetric stretching vibration of free dien molecules to 3217 cm−1 for that of the hybrid rods, which correspond to the chemical coordination of –NH2 groups with Fe2+ ions in the present hybrid rods.
TGA and dWeight/dT curves in Figure 3 show a weight loss (~6.7 wt%) from room temperature to the onset decomposition temperature (Tonset) ~540 K due to a small amount of free dien and other organic solvents absorbed on the surface of the hybrid rods. The Tonset value is obviously higher than that of the previously reported (Fe0.86Se2)2Fe(dien)2 [22]. Between 540 K and ~585 K, a sharp weight loss of about 15.9 wt% should be ascribed to releasing the bonded dien from the hybrid rods, while a slow weight loss (5.3 wt%) between 585 K and the end temperature (Tend) of ~700 K is due to the loss of the left dien and a small amount of Se. To obtain a precise content of dien in the hybrid rods, we performed the experiments as follows: At first, clean Al2O3 crucibles were calcined to 1100 K for 24 h in an air atmosphere. The Al2O3 crucibles were used to contain the hybrid rods for the subsequent thermal decomposition. The masses of an Al2O3 crucible and the hybrid rods were weighed together at different steps. The mass of the Al2O3 crucible was deducted for convenience. The hybrid rods with an initial mass of 68.6 mg were slowly heated to 580 K in an Ar flow for 24 h, at which temperature the hybrid rods were completely decomposed through releasing coordinated dien but without losing Se atoms from the decomposed product. The mass of the decomposition product was 51.1 mg. Therefore, the weight loss was determined to be about 25.4 wt%, which is smaller than the total weight loss obtained by TGA without loss of Se. If we subtract the loss of free dien and other organic solvents absorbed on the surface of the hybrid rods, the loss of coordinated dien should be about 18.7 wt%. Taking into account that there are 18.7 g of dien and 74.6 g of inorganic Fe3.25Se4 in 100 g of hybrid rods, the molar ratio y between dien to Fe3.25Se4 in the hybrid rods could be calculated by the equation:
y = 18.7 / M d i e n 74.6 / M Fe 3.25 Se 4 ,
where M dien and M Fe 3.25 Se 4 are the molecular weights of the organic component (dien) and the inorganic component (Fe3.25Se4), respectively. The y for the hybrid rods is ~1.2 and the formula of the hybrid rods is determined as (Fe3.25Se4)(dien)1.2.
Powder XRD pattern of the hybrid rods (Figure 4) reveals that all Bragg diffraction peaks can be refined and indexed by using the monoclinic structure with the space group P21/c (14). The corresponding refinement process gave good R factors (Rp = 8.52%, Rwp = 7.45% and χ2 = 2.72), and refined room-temperature lattice parameters of the hybrid material are a = 11.397(7) Å, b = 19.376(3) Å, c = 11.185(6) Å and β = 105.04°. The crystal structure of the hybrid rods is the same as that for Fe3Se4(tren) (tren = tris(2-aminoethyl)amine) [13] but different from those for previous orthorhombic Fe3Se4(dien)2 [13] and iron vacancy doped (Fe0.86Se2)2Fe(dien)2 [22], in which two independent subsystems have been identified: 1D FeSe2 chains and Fe(dien)2 complex. Because two dien molecules with six nitrogen atoms have bonded well with a Fe2+ to form a [Fe(dien)]2+ complex, the Fe(dien)2 complex should be the only organic fragment for the orthorhombic Fe3Se4(dien)2 [13] and the monoclinic hybrid rods. Therefore, a change of crystal structure from the orthorhombic Fe3Se4(dien)2 [13] to the present monoclinic hybrid rods should be ascribed to a bit increase of Fe atoms in the inorganic fragment of hybrid rods. The Fe2Se3 superstructure is the closest fragment to FeSe2 in chemical composition [23]. Therefore, a formula of the hybrid rods may be written as (Fe1.99Se3)2[Fe(dien)2]0.9. Taking into account two independent subsystems consisting of the (Fe2Se3)2− double chains and the Fe2+(dien)2 complexes, there are both Fe3+ and Fe2+ ions in the hybrid rods similar to the case of the orthorhombic Fe3Se4(dien)2 [13]. Figure 5 represents the Fe L-edge X-ray absorption spectrum (XAS) line of the monoclinic hybrid rods in total electron yield (TEY) mode, along with that of commercial Fe3O4 as a reference for Fe3+ and Fe2+ oxidation states. As a guide to the valence states, the line shapes of the sample are compared with that of reference, indicating the signatures of Fe3+ and Fe2+. This reveals that there are both trivalent and bivalent Fe ions in the as-synthesized monoclinic hybrid rods. It should be noted that information on the monoclinic hybrid phase was seldom mentioned in the previous transition-metal chalcogenides-dien systems [13,17,20,22,30,31,32,33].

3.2. Growth Mechanism

Similar to the Fe vacancies doped orthorhombic hybrid cuboids [22], the monoclinic hybrid rods have been synthesized by using soluble iron and selenium precursors and organic dien. Although inorganic FeSex building blocks, such as 1D FeSe2 chains and 2D β-Fe3Se4 layers, play an important role in the formation of the FeSex-amine hybrid materials [13,17,20,22], there is no precise information on how the 1D FeSe2 chains change to the 2D β-Fe3Se4 layers. In the solution syntheses, the dien molecules should play three important roles in the solvent, the reductive agent and the precursor at the same time [22]. Se atoms and a part of Fe3+ ions can be reduced by dien to Se2− ions and Fe2+ ions, respectively. Meanwhile, the redox reactions produce nitrogen, serving as the production of the oxidation [21,34]. Based on a bottom-up growth mechanism, Figure 6 illustrates three combination modes of organic Fe(dien)2 complexes with (I) 1D FeSe2 chains, (II) Fe2Se3 double chains and (III) 2D β-Fe3Se4 layers, respectively, in the present reaction system, following the reaction formulas:
Fe2+ + 2dien = Fe2+(dien)2
Fe3+ + 2Se2− = [FeSe2]
2Fe3+ + 4Se2− + Fe2+ + 2dien = [FeSe2]2[Fe(dien)2]
3[FeSe2]2[Fe(dien)2] + 0.75Fe2+ = 2[Fe2Se3]2[Fe(dien)2]0.875 + 2.5dien
The Fe2+(dien)2 complexes are formed by coordinating the Fe2+ ions with dien molecules, while the FeSe2 chains are initially created by the reaction of Se2− and Fe3+ ions, following the reaction formulas (1) and (2). Combinations of FeSe2 chains and Fe2+(dien)2 complexes are driven by the Se∙∙∙H–N interactions due to strong electronegativity of Se atoms [22]. Therefore, the synthesis of orthorhombic [FeSe2]2[Fe(dien)2] with a cuboid shape can be proposed as the growth model (I) through a self-assembly reaction of 1D FeSe2 chains and Fe2+(dien)2 complexes following the reaction formula (3). The powder XRD pattern of the hybrid cuboids (Figure 7a) indicates that all Bragg diffraction peaks can be refined and indexed by using the orthorhombic structure with the space group C2221 (No. 20). Such an XRD pattern reveals the same crystal structure as that of Fe3Se4(dien)2 [13]. The corresponding refinement process gave good R factors (Rp = 18.3%, Rwp = 18.7% and χ2 = 6.48) for the hybrid cuboids. Refined lattice parameters at room temperature of the hybrid cuboids are 9.226(6) Å for a axis, 18.000(0) Å for b axis, and 11.610(7) Å for c axis, about 0.94% and 0.58% expansion along the a and c axes and 0.67% shrinkage along the b axis when compared with those of Fe3Se4(dien)2 [13]. The orthorhombic hybrid particles are in the paramagnetism in good agreement with previous Fe3Se4(dien)2 [13]. The magnetic properties are not shown here.
Given the redox reaction system at a higher temperature (503 K), Fe3+ ions are preferably reduced to Fe2+ ions. When the molar ratio of Fe and Se atoms in the starting materials changes from 3:4 to 3.25:4, a diffusion of more iron atoms into the orthorhombic [FeSe2]2[Fe(dien)2] would occur following the reaction formula (4), resulting in the monoclinic hybrid rods (Figure 4). A reasonable molecular formula for the hybrid rods is proposed as [ Fe 1.125 3 + Fe 0.875 2 + Se 3 2 ]2[ Fe 2 + (dien)2]0.875 according to electrical neutrality principles. The content of 0.875 dien/cell is obtained by balancing chemical Equation (4), which is almost the same as the experimental value of 0.9 dien/cell for the present hybrid rods determined above. Assuming that the small difference between the calculated and the experimental values is in range of the analytical error, we propose that the monoclinic hybrid rods are built by Fe2Se3 double chains and Fe(dien)2 complexes in the model (II).
Moreover, further increases in the molar ratio of Fe and Se to 3.5:4 and the reaction temperature to 513 K result in the hybrid nanoplates. Figure 8 shows the morphology transformation from particles for the orthorhombic phase to rods for the monoclinic phase and plates for the (Fe3.5Se4)-dien. Figure 7b presents the XRD pattern of (Fe3.5Se4)-dien hybrid plates. Two strong peaks at low 2θ angles of 8.48° and 17.00° with lattice spacings of 10.42 and 5.21 Å reveal the presence of period inorganic layers separated by the Fe(dien)2 complex, similar to previous hybrid plates with a tetragonal β-Fe3Se4 superstructure [20] and an inorganic Fe0.9Co0.1S1.2 unit [31]. Because the hybrid plates are mixed by an impurity of FexSe with an uncertain quality, the formula for the hybrid phase is not determined by the same method for the hybrid rods. However, an ordered tetragonal superstructure is determined in the presence of the hybrid plates by a SAED image (the inset of Figure 8d), which is similar to that of the inorganic Fe0.9Co0.1S1.2 unit [31] and the tetragonal β-Fe3Se4 superstructure [20]. Taking into account the composition, this ordered superstructure is suggested as the tetragonal β-Fe3Se4. Therefore, the growth model (III) can be illustrated by the combination of the inorganic tetragonal β-Fe3Se4 superstructures and the Fe(dien)2 complexes for the synthesis of hybrid nanoplates in the iron selenide-dien hybrid system. Efforts to examine the crystal structure of (Fe3.5Se4)-dien hybrid plates are currently in progress.
As shown in Figure 6, varied inorganic building units are key factors for syntheses of corresponding hybrid products, which depend on the Fe/Se stoichiometry and the reacting temperatures. In the solution reaction system, iron-diffusion reactions, such as the reaction formulas (3) and (4), are driven by different reaction temperatures. Figure 4 reveals a single phase of hybrid rods with a monoclinic structure, which is built by Fe2Se3 double chains and Fe(dien)2 complexes at a molecular level and in a controllable manner. An improper reaction condition will result in mixtures of several hybrid materials but not a single phase.

3.3. Magnetic Properties

Figure 9 represents the magnetic properties of the monoclinic hybrid rods. In contrast to the stoichiometric [FeSe2]2[Fe(dien)2] that is paramagnetic [13], the temperature dependence of the magnetization in the FC process for the monoclinic hybrid rods shows a magnetic transition at the Curie temperature (TC) of 11 K (inset of Figure 9). The TC value is determined by the point of intersection of the two tangents around the inflection point of the FC magnetization curve. Such a TC value is much lower than that of the iron vacancy doped (Fe0.86Se2)2Fe(dien)2 [22], revealing that the ferrimagnetism is independent on the uncompensated magnetic iron ions. There is no magnetic transition above 11 K, suggesting that the origin of ferrimagnetic behavior of this hybrid material could not be caused by traces of ferromagnetic impurity Fe3O4 with the TC of about 860 K and ferrimagnetic iron selenides, such as Fe3Se4 and Fe7Se8. It is well known that the TC values for Fe3Se4 and Fe7Se8 are about 320 K [35] and 450 K [36], respectively. The magnetic hysteresis loops of the hybrid rods in Figure 9 further exhibit the ferromagnetic feature in a temperature ranging from 2 to 10 K. The magnetization at 50 kOe (M50) and coercivity of the hybrid rods are 13.6 emu/g and 4.67 kOe, respectively, at 2 K. Such a M50 of the hybrid rods is obviously larger than the saturation magnetization value of 5.6 emu/g for ferromagnetic (CH3NH3)2CuCl4 at 10 K [7], of 6 emu/g for FIM [Fe14Se16](tepa) hybrid plates at 10 K [29] and 0.01 emu/g for (NH3–CH2–C6H4CO2H)[SnCl6] at 300 K [21]. Moreover, the high coercivity of the hybrid rods is rare in organic–inorganic hybrid materials, for example, 30 Oe for the (PEA)2CuCl4 (PEA = C6H5C2H4NH3) film at 5 K [9], 404 Oe for the (NH3–CH2–C6H4CO2H)[SnCl6] at 300 K [21], 1.5 kOe for TBA intercalated NiPS3 (TBA = tetrabutylammonium) at 5 K and 2.2 kOe for cobaltocenium ions (Co(Cp)2+ (Cp = cyclopentadienyl ring C5H5) intercalated NiPS3 at 5 K [24]. We suggest that the large coercivity results from large uniaxial magnetocrystalline anisotropy of the hybrid rods [37]. As the temperature rises, the coercivity significantly decreases to 1.65 kOe at 5 K and about 20 Oe at 10 K. It is obvious that the magnetic field dependence of magnetization is in the ferromagnetic characteristics in a low magnetic field range, but in a linear magnetization in the high magnetic field range. The linear magnetization curves in the high field range may indicate the existence of a paramagnetic or antiferromagnetic component because of the nonsaturation feature, even at the magnetic field of 50 kOe. Such a linear magnetization process was ascribed to either weakened sublattice or intersublattice spins disoriented by thermal motion [35] or the noncollinear spin alignments in the magnetic system. The linear field dependence of the magnetization at higher fields is not contrary to the FIM compounds, in which strong antiferromagnetic coupling between different magnetic sublattices prevents their full alignment by the magnetic field [20]. The remanant magnetization (Mr) is 8 emu/g at 2 K, which results in a good magnetic remanence ratio (Mr/M50) of ~0.6. The excellent magnetic properties may be ascribed to the quasi-one-dimensional Fe2Se3 double chains in the hybrid rods, which is potential to be applied in the new type of permanent magnets.
Quasi-1D spin-ladder compounds, such as MFe2Se3 (M = Ba, Cs) [25,26,27,28], have attracted considerable interest. Either block magnetism [25] or stripelike magnetism [27] was proposed as the magnetic origins of these ladder compounds, where the magnetic moments couple ferromagnetically (or antiferromagnetically) along the rung (or the leg) direction. Because spin ladders in copper oxides shed light on the mechanism of superconductivity, a study on an analog with ladder geometry among ferrous compounds is highly interesting. It is obvious that all the iron atoms in BaFe2Se3 are ferric, while those in CsFe2Se3 are composed of ferric and ferrous ions with a molar ratio of 1:1. In our case, the molecular formula of [ Fe 1.125 3 + Fe 0.875 2 + Se 3 2 + ]2[ Fe 2 + (dien)2]0.875 reveals the iron composition, which enables creation of a magnetic structure that is different from those for the antiferromagnetic BaFe2Se3 and CsFe2Se3 due to the varied content of ferric and ferrous ions. This monoclinic hybrid material has been classified by the large magnetization and coercivity at 2 K as a ferrimagnetic compound. In comparison with the Fe3Se4(dien)2 with 1D Fe 3 + Se 2 2 + single chains [13], the ferric and ferrous ions in Fe 1.125 3 + Fe 0.875 2 + Se 3 2 double chains should be responsible for the ferrimagnetic interactions. Moreover, we easily see that the Fe 1.125 3 + Fe 0.875 2 + Se 3 2 double chains in present hybrid rods are different from Fe 2 3 + Se 3 2 in BaFe2Se3 and Fe 3 + Fe 2 + Se 2 2 in CsFe2Se3. Due to a diffusing reaction in the formation of [ Fe 1.125 3 + Fe 0.875 2 + Se 3 2 ]2[ Fe 2 + (dien)2]0.875, the distributions of Fe3+ and Fe2+ in the Fe 1.125 3 + Fe 0.875 2 + Se 3 2 double chains are not clear. Efforts to examine the magnetic structure of [Fe2Se3]2[Fe(dien)2]0.9 hybrid rods with determined atom coordinates are currently in progress.

4. Conclusions

We developed a facile protocol for bottom-up synthesizing organic–inorganic hybrid materials by connecting inorganic fragments of FeSe2 single chains, Fe2Se3 double chains or β-FexSe layers with Fe(dien)2 complexes. These materials possess varied crystal structures and magnetic properties. Of note, the monoclinic (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods with the space group P21/c (14) are ferrimagnetic and the Curie temperature (TC) is determined to be ~11 K. The hybrid rods show a high coercivity (HC) of 4.67 kOe and a saturated magnetization (MS) of 13.5 emu/g at 2 K, which should be ascribed to the ferrimagnetic coupling between the organic Fe(dien)2 complexes and inorganic Fe2Se3 double chains. Large coercivity and magnetic remanence ratios make the monoclinic hybrid rods an excellent organic permanent magnet.

Author Contributions

Conceptualization, D.L.; methodology, D.L.; investigation, X.S., Q.K., X.M. and S.L.; formal analysis, X.S.; resources, D.L. and Z.Z.; data curation, X.S.; writing—original draft preparation, X.S. and D.L.; writing—review and editing, D.L. and Z.Z.; supervision, D.L. and Z.Z. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of China under Grant No. 51971221, 52031014 and by the National Key R&D Program of China (No. 2017YFA0700702) from the ministry of Science and Technology of China.

Data Availability Statement

The data are available upon reasonable request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Wei, M.M.; Fan, Y.C.; Qin, W. Progress of organic magnetic materials. Sci. China Phys. Mech. 2019, 62, 977501. [Google Scholar] [CrossRef]
  2. Sanchez, C.; Julian, B.; Belleville, P.; Popall, M. Applications of hybrid organic-inorganic nanocomposites. J. Mater. Chem. 2005, 15, 3559–3592. [Google Scholar]
  3. Welbes, L.L.; Borovik, A.S. Confinement of metal complexes within porous hosts: Development of functional materials for gas binding and catalysis. Acc. Chem. Res. 2005, 38, 765–774. [Google Scholar] [CrossRef]
  4. Ansari, F.; Ding, Y.C.; Berglund, L.A.; Dauskardt, R.H. Toward sustainable multifunctional coatings containing nanocellulose in a hybrid glass matrix. ACS Nano 2018, 12, 5495–5503. [Google Scholar] [CrossRef]
  5. Li, W.; Xia, F.; Qu, J.; Li, P.; Chen, D.H.; Chen, Z.; Yu, Y.; Lu, Y.; Caruso, R.A.; Song, W.G. Versatile inorganic-organic hybrid WOx-ethylenediamine nanowires: Synthesis, mechanism and application in heavy metal ion adsorption and catalysis. Nano Res. 2014, 7, 903–916. [Google Scholar] [CrossRef]
  6. Jin, S.F.; Fan, X.; Wu, X.Z.; Sun, R.J.; Wu, H.; Huang, Q.Z.; Shi, C.L.; Xi, X.K.; Li, Z.L.; Chen, X.L. High-TC superconducting phases in organic molecular intercalated iron selenides: Synthesis and crystal structures. Chem. Commun. 2017, 53, 9729–9732. [Google Scholar] [CrossRef] [PubMed]
  7. Zhao, H.Y.; Fu, H.R.; Hu, Z.; Fu, Q.M.; Tao, H.; Weng, J.; Xiong, L.W.; Cheng, Z.X. Magnetic hybrid organic-inorganic perovskite (CH3NH3)2XCl4 (X = Mn, Cu, Co) crystals. CrystEngComm 2021, 23, 5208–5213. [Google Scholar] [CrossRef]
  8. Asensio, Y.; Marras, S.; Spirito, D.; Gobbi, M.; Ipatov, M.; Casanova, F.; Mateo-Alonso, A.; Hueso, L.E.; Martin-Garcia, B. Magnetic properties of layered hybrid organic-inorganic metal-halide perovskites: Transition metal, organic cation and perovskite phase effects. Adv. Funct. Mater. 2022, 32, 2207988. [Google Scholar] [CrossRef]
  9. Kim, K.Y.; Park, G.; Cho, J.; Kim, J.; Kim, J.S.; Jung, J.; Park, K.; You, C.Y.; Oh, I.H. Intrinsic magnetic order of chemically exfoliated 2D ruddlesden-popper organic-inorganic halide perovskite ultrathin films. Small 2020, 16, 2005445. [Google Scholar] [CrossRef]
  10. Zhang, S.L.; Li, X.C.; Gu, S.Y.; Guo, S.; Liu, Z.Y.; Zeng, S.Y.; Li, S.S. Crystal structures and magnetic properties of one-dimensional compounds constructed from Mn2(salen)2 building blocks and organic selenite acid ligands. N. J. Chem. 2021, 45, 21599–21605. [Google Scholar] [CrossRef]
  11. Sibille, R.; Mazet, T.; Diop, L.V.B.; Francois, M. Crystal structure and magnetic properties of the layered hybrid organic-inorganic compounds M2(OH)2(C14H8O4) (M = Mn, Fe). Acta Crystallogr. Sect. B 2021, 77, 801–807. [Google Scholar] [CrossRef]
  12. Gao, M.R.; Yao, W.T.; Yao, H.B.; Yu, S.H. Synthesis of unique ultrathin lamellar mesostructured CoSe2-amine (protonated) nanobelts in a binary solution. J. Am. Chem. Soc. 2009, 131, 7486–7487. [Google Scholar] [CrossRef]
  13. Greenfield, J.T.; Pak, C.; Kamali, S.; Lee, K.; Kovnir, K. Control over connectivity and magnetism of tetrahedral FeSe2 chains through coordination Fe-amine complexes. Chem. Commun. 2015, 51, 5355–5358. [Google Scholar] [CrossRef] [PubMed]
  14. Zheng, Y.Z.; Xue, W.; Zheng, S.L.; Tong, M.L.; Chen, X.M. Néel temperature enhancement by increasing the in-plane magnetic correlation in layered inorganic-organic hybrid materials. Adv. Mater. 2008, 20, 1534–1538. [Google Scholar] [CrossRef]
  15. De Luis, R.F.; Urtiaga, M.K.; Mesa, J.L.; Vidal, K.; Lezama, L.; Rojo, T.; Arriortua, M.I. Short-range and long-range magnetic ordering, in third generation brannerite type inorganic–organic-vanadates: [{Mn(Bpy)}(VO3)2] approximate to (H2O)1.16 and [{Mn(Bpy)0.5}(VO3)2] approximate to (H2O)0.62. Chem. Mater. 2010, 22, 5543–5553. [Google Scholar] [CrossRef]
  16. Kurmoo, M.; Kumagai, H.; Green, M.A.; Lovett, B.W.; Blundell, S.J.; Ardavan, A.; Singleton, J. Two modifications of layered cobaltous terephthalate: Crystal structures and magnetic properties. J. Solid State Chem. 2001, 159, 343–351. [Google Scholar] [CrossRef]
  17. Pak, C.; Kamali, S.; Pham, J.; Lee, K.; Greenfield, J.T.; Kovnir, K. Chemical excision of tetrahedral FeSe2 chains from the superconductor FeSe: Synthesis, crystal structure, and magnetism of Fe3Se4(en)2. J. Am. Chem. Soc. 2013, 135, 19111–19114. [Google Scholar] [CrossRef] [Green Version]
  18. Zang, Z.-A.; Yao, H.-B.; Zhou, Y.-X.; Yao, W.-T.; Yu, S.-H. Synthesis and magnetic properties of new [Fe18S25](TETAH)14 (TETAH = protonated triethylenetetramine) nanoribbons: An efficient precursor to Fe7S8 nanowires and porous Fe2O3 nanorods. Chem. Mater. 2008, 20, 4749–4755. [Google Scholar] [CrossRef]
  19. Kuang, Q.; Men, X.; Shang, X.; Yang, B.; Zhou, Y.; Zhang, B.; Li, Z.; Li, D.; Zhang, Z. Magnetism of tetragonal β-Fe3Se4 nanoplates controllably synthesized by thermal decomposition of (β-Fe2Se3)4[Fe(tepa)] hybrid. Magnetism 2022, 2, 31–44. [Google Scholar] [CrossRef]
  20. Pan, D.S.; Li, Y.; Han, Z.; Li, B.; Wang, C.W.; Yang, T.; Li, D.; Choi, C.K.; Zhang, Z.D. Organic-inorganic hybrid (β-Fe3Se4)4[Fe(teta)1.5] (teta = triethylenetetramine) nanoplates: Solution synthesis and magnetic properties. Chem. Mater. 2018, 30, 8975–8982. [Google Scholar] [CrossRef]
  21. Kaiba, A.; Al Otaibi, F.; Geesi, M.H.; Riadi, Y.; Aljohani, T.A.; Guionneau, P. A new organic-inorganic hybrid compound (NH3(CH2)C6H4CO2H)[SnCl6]: Synthesis, crystal structure, vibrational, optical, magnetic properties and theoretical study. J. Mol. Struct. 2021, 1234, 130129. [Google Scholar] [CrossRef]
  22. Pan, D.S.; Kuang, Q.F.; Tong, P.; Tong, W.; Fan, L.B.; Zhao, J.; Li, D.; Choi, C.J.; Zhang, Z.D. Self-assembly of 1D FeSe2 chains and Fe(dien)2 complexes for ferrimagnetic inorganic-organic hybrid cuboids. J. Magn. Magn. Mater. 2022, 542, 168585. [Google Scholar] [CrossRef]
  23. Chen, T.K.; Chang, C.C.; Chang, H.H.; Fang, A.H.; Wang, C.H.; Chao, W.H.; Tseng, C.M.; Lee, Y.C.; Wu, Y.R.; Wen, M.H.; et al. Fe-vacancy order and superconductivity in tetragonal β-Fe1-xSe. Proc. Natl. Acad. Sci. USA 2014, 111, 63–68. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  24. Tezze, D.; Pereira, J.M.; Asensio, Y.; Ipatov, M.; Calavalle, F.; Casanova, F.; Bittner, A.M.; Ormaza, M.; Martin-Garcia, B.; Hueso, L.E.; et al. Tuning the magnetic properties of NiPS3 through organic-ion intercalation. Nanoscale 2022, 14, 1165–1173. [Google Scholar] [CrossRef]
  25. Nambu, Y.; Ohgushi, K.; Suzuki, S.; Du, F.; Avdeev, M.; Uwatoko, Y.; Munakata, K.; Fukazawa, H.; Chi, S.; Ueda, Y.; et al. Block magnetism coupled with local distortion in the iron-based spin-ladder compound BaFe2Se3. Phys. Rev. B 2012, 85, 064413. [Google Scholar] [CrossRef] [Green Version]
  26. Lei, H.; Ryu, H.; Frenkel, A.I.; Petrovic, C. Anisotropy in BaFe2Se3 single crystals with double chains of FeSe tetrahedra. Phys. Rev. B 2011, 84, 214511. [Google Scholar] [CrossRef] [Green Version]
  27. Du, F.; Ohgushi, K.; Nambu, Y.; Kawakami, T.; Avdeev, M.; Hirata, Y.; Watanabe, Y.; Sato, T.J.; Ueda, Y. Stripelike magnetism in a mixed-valence insulating state of the Fe-based ladder compound CsFe2Se3. Phys. Rev. B 2012, 85, 214436. [Google Scholar] [CrossRef]
  28. Krzton-Maziopa, A.; Pomjakushina, E.; Pomjakushin, V.; Sheptyakov, D.; Chernyshov, D.; Svitlyk, V.; Conder, K. The synthesis, and crystal and magnetic structure of the iron selenide BaFe2Se3 with possible superconductivity at Tc = 11 K. J. Phys. Condens. Matter. 2011, 23, 402201. [Google Scholar] [CrossRef] [Green Version]
  29. Da Li, Q.K.; Men, X.; Zhang, B.; Shang, X.; Yang, B.; Yang, T.; Li, Z.; Zhang, Z. High-temperature superconductivity (TC = 42 K) of Fe1.2[Fe(tepa)]0.8(β-Fe3Se4)4. Research Square 2022. Preprint (Version 1). [Google Scholar] [CrossRef]
  30. Hua, A.; Zhou, W.Y.; Li, Y.; Li, S.Z.; Cheng, R.F.; Yang, J.X.; Luan, J.; Wang, X.H.; Jiang, C.H.; Li, D.; et al. A novel strategy for synthesizing the large size Co9S8@C nanosheets as anode for lithium-ion batteries with superior performance. J. Alloys Compd. 2022, 895, 162668. [Google Scholar] [CrossRef]
  31. Pan, D.S.; Xiao, B.; Wang, Q.; Wang, H. Chemical conversion synthesis of magnetic Fe1-xCox alloy nanosheets with controlled composition. Chem. Commun. 2021, 57, 2309–2312. [Google Scholar] [CrossRef] [PubMed]
  32. Yao, W.T.; Yu, S.H.; Huang, X.Y.; Jiang, J.; Zhao, L.Q.; Pan, L.; Li, J. Nanocrystals of an inorganic-organic hybrid semiconductor: Formation of uniform nanobelts of [ZnSe](diethylenetriamine)0.5 in a ternary solution. Adv. Mater. 2005, 17, 2799–2802. [Google Scholar] [CrossRef]
  33. Zhang, M.; Shi, C.; Zhang, T.K.; Feng, M.; Chang, L.; Yao, W.T.; Yu, S.H. Mn-substituted [Zn1−xMnxSe](DETA)0.5 (x = 0–0.3) inorganic-organic hybrid nanobelts: Synthesis, electron paramagnetic resonance spectroscopy, and their temperature- and pressure-dependent optical properties. Chem. Mater. 2009, 21, 5485–5490. [Google Scholar] [CrossRef]
  34. Li, Y.; Kuang, Q.F.; Men, X.L.; Wang, S.G.; Li, D.; Choi, C.J.; Zhang, Z.D. Anisotropic growth and magnetic properties of α″-Fe16N2@C nanocones. Nanomaterials 2021, 11, 890. [Google Scholar] [CrossRef]
  35. Aliev, N.G.; Guseinov, N.G.; Kerimov, I.G.; Sadykhov, R.Z.; Guseinov, D.A. Magnetic-properties of Fe3Se4. Inorg. Mater. 1977, 13, 519–521. [Google Scholar]
  36. Kamimura, T.; Kamigaki, K.; Hirone, T.; Sato, K. On Magnetocrystalline Anisotropy of Iron Selenide Fe7Se8. J. Phys. Soc. Jpn. 1967, 22, 1235–1240. [Google Scholar] [CrossRef]
  37. Long, G.; Zhang, H.W.; Li, D.; Sabirianov, R.; Zhang, Z.D.; Zeng, H. Magnetic anisotropy and coercivity of Fe3Se4 nanostructures. Appl. Phys. Lett. 2011, 99, 202103. [Google Scholar] [CrossRef]
Figure 1. (a,b) SEM images and (c) the corresponding EDX spectrum of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods. (d) Typical TEM image of a single hybrid rod. Inset shows the corresponding SAED pattern. (e) A STEM image and corresponding element mapping of (f) Fe, (g) Se, (h) C and (i) N for a single (Fe2Se3)2[Fe(dien)2]0.9 hybrid rod.
Figure 1. (a,b) SEM images and (c) the corresponding EDX spectrum of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods. (d) Typical TEM image of a single hybrid rod. Inset shows the corresponding SAED pattern. (e) A STEM image and corresponding element mapping of (f) Fe, (g) Se, (h) C and (i) N for a single (Fe2Se3)2[Fe(dien)2]0.9 hybrid rod.
Nanomaterials 13 00487 g001
Figure 2. FTIR spectrum of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods. The inset shows the vibration bands of –CH2–, –NH2, and –CN–.
Figure 2. FTIR spectrum of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods. The inset shows the vibration bands of –CH2–, –NH2, and –CN–.
Nanomaterials 13 00487 g002
Figure 3. TGA and dWeight/dT curves of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods.
Figure 3. TGA and dWeight/dT curves of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods.
Nanomaterials 13 00487 g003
Figure 4. Powder XRD pattern of (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods recorded at room temperature (solid crosses) with Rietveld refinements and difference curves.
Figure 4. Powder XRD pattern of (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods recorded at room temperature (solid crosses) with Rietveld refinements and difference curves.
Nanomaterials 13 00487 g004
Figure 5. XAS of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods and Fe3O4 as reference. The main peak of Fe L3-absorption edge is at 710 eV with lower shoulder at 708 eV, and the main peak of Fe L2-absorption edge is at 720 eV with higher shoulder at 722 eV.
Figure 5. XAS of the (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods and Fe3O4 as reference. The main peak of Fe L3-absorption edge is at 710 eV with lower shoulder at 708 eV, and the main peak of Fe L2-absorption edge is at 720 eV with higher shoulder at 722 eV.
Nanomaterials 13 00487 g005
Figure 6. Schematic illustration of combining organic Fe(dien)2 complexes with (I) 1D FeSe2 chains, (II) Fe2Se3 double chains and (III) 2D FexSe layers, respectively, for the syntheses of three hybrid phases at different reaction conditions.
Figure 6. Schematic illustration of combining organic Fe(dien)2 complexes with (I) 1D FeSe2 chains, (II) Fe2Se3 double chains and (III) 2D FexSe layers, respectively, for the syntheses of three hybrid phases at different reaction conditions.
Nanomaterials 13 00487 g006
Figure 7. Powder XRD patterns of (a) [FeSe2]2[Fe(dien)2] particles and (b) (Fe3.5Se4)-dien plates.
Figure 7. Powder XRD patterns of (a) [FeSe2]2[Fe(dien)2] particles and (b) (Fe3.5Se4)-dien plates.
Nanomaterials 13 00487 g007
Figure 8. Microstructure of (a) [FeSe2]2[Fe(dien)2] hybrid particles, (b) (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods, (c) an intermediate product between the rodlike and the platelike samples and (d) a (Fe3.5Se4)-dien hybrid plate. Inset shows the corresponding SAED pattern obtained perpendicular to the nanoplate marked by the red circle.
Figure 8. Microstructure of (a) [FeSe2]2[Fe(dien)2] hybrid particles, (b) (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods, (c) an intermediate product between the rodlike and the platelike samples and (d) a (Fe3.5Se4)-dien hybrid plate. Inset shows the corresponding SAED pattern obtained perpendicular to the nanoplate marked by the red circle.
Nanomaterials 13 00487 g008
Figure 9. Hysteresis loops of (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods measured at different temperatures. Inset shows temperature dependence of FC magnetizations in a magnetic field H = 100 Oe.
Figure 9. Hysteresis loops of (Fe2Se3)2[Fe(dien)2]0.9 hybrid rods measured at different temperatures. Inset shows temperature dependence of FC magnetizations in a magnetic field H = 100 Oe.
Nanomaterials 13 00487 g009
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Shang, X.; Men, X.; Kuang, Q.; Li, S.; Li, D.; Zhang, Z. Controllable Connection of Fe2Se3 Double Chains and Fe(dien)2 Complexes for Organic–Inorganic Hybrid Ferrimagnet with a Large Coercivity. Nanomaterials 2023, 13, 487. https://doi.org/10.3390/nano13030487

AMA Style

Shang X, Men X, Kuang Q, Li S, Li D, Zhang Z. Controllable Connection of Fe2Se3 Double Chains and Fe(dien)2 Complexes for Organic–Inorganic Hybrid Ferrimagnet with a Large Coercivity. Nanomaterials. 2023; 13(3):487. https://doi.org/10.3390/nano13030487

Chicago/Turabian Style

Shang, Xiaolei, Xiaoling Men, Qifeng Kuang, Shaojie Li, Da Li, and Zhidong Zhang. 2023. "Controllable Connection of Fe2Se3 Double Chains and Fe(dien)2 Complexes for Organic–Inorganic Hybrid Ferrimagnet with a Large Coercivity" Nanomaterials 13, no. 3: 487. https://doi.org/10.3390/nano13030487

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop