Next Article in Journal
The Influence of Nanostructured Alumina Coating on Bonding and Optical Properties of Translucent Zirconia Ceramics: In Vitro Evaluation
Next Article in Special Issue
Ferroelectric and Ferroelastic Domain Related Formation and Influential Mechanisms of Vapor Deposited Piezoelectric Thin Films
Previous Article in Journal
Self-Aligned Thin-Film Patterning by Area-Selective Etching of Polymers
Previous Article in Special Issue
Synthesis, Microstructure and Properties of Magnetron Sputtered Lead Zirconate Titanate (PZT) Thin Film Coatings
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Exchange Bias Effect in LaFeO3: La0.7Ca0.3MnO3 Composite Thin Films

1
Department of Vehicle Engineering, Changzhou Vocational Institute of Mechatronic Technology, Changzhou 213164, China
2
Qingdao Special Service Sanatorium of PLA Navy, Qingdao 266000, China
3
Key Laboratory for Precision and Non-Traditional Machining Technology of the Ministry of Education, Dalian University of Technology, Dalian 116024, China
4
Institute of Oceanographic Instrumentation, Qilu University of Technology (Shandong Academy of Science), Qingdao 266001, China
5
School of Materials, Sun Yat-sen University, Guangzhou 510275, China
*
Authors to whom correspondence should be addressed.
These authors contribute equally to this work.
Coatings 2021, 11(9), 1125; https://doi.org/10.3390/coatings11091125
Submission received: 31 August 2021 / Revised: 7 September 2021 / Accepted: 10 September 2021 / Published: 16 September 2021
(This article belongs to the Special Issue Nanocomposite Thin Film and Multilayers)

Abstract

:
Composite thin films arouse great interests owing to the multifunctionalities and heterointerface induced physical property tailoring. The exchange bias effect aroused from the ferromagnetic (FM)–antiferromagnetic (AFM) heterointerface is applicable in various applications such as magnetic storage. In this work, (LaFeO3)x:(La0.7Ca0.3MnO3)1−x composite thin films have been deposited via pulsed laser deposition (PLD) and the exchange bias effect was investigated. In such system, LaFeO3 (LFO) is an antiferromagnet while La0.7Ca0.3MnO3 (LCMO) is a ferromagnet, which results in the exchange bias interfacial coupling at the FM/AFM interface. The composition variation of the two phases could lead to the exchange bias field (HEB) tuning in the composite system. This work demonstrates a new composite thin film system with FM-AFM interfacial exchange coupling, which could be applied in various spintronic applications.

1. Introduction

Exchange bias (EB) describes the pinning of the magnetic dipoles due to the interfacial exchange coupling between ferromagnetic (ferrimagnetic, FM) and antiferromagnetic (AFM) components after cooling through Néel temperature (TN) of the antiferromagnets, which results in the shift of the hysteresis loop. The EB field (HEB) is used to evaluate the EB effect, which could be defined as HEB = |H+ + H|/2, where H+ and H are the positive and negative coercivity in the hysteresis loop, respectively. The EB phenomenon was first observed in the AFM CoO nanoparticle wrapped by an FM Co shell, reported by Meiklejohn and Bean in 1956, and the Meiklejohn–Bean model has been widely accepted to explain the mechanism of EB effect [1]. The EB effect could be employed in a lot of applications, such as magnetoresistive read heads, magnetic sensors, spin valve devices, as well as high-density data storage [2,3,4,5]. Thus far, the EB effect has been realized in various material systems and geometries, such as granular composites, core–shell nanoparticles, nanocluster arrays with capping layer and thin films [6,7,8,9].
Among all the different nanostructures with EB effect, the thin film form might be the most promising for practical applications, and a tremendous research effort has been devoted to exploring the EB effect in thin films. Typically, the FM/AFM exchange coupling in thin film could be achieved in the following forms: multilayer thin film, vertically aligned nanocomposite thin film, solid solution (or composite) thin film or even a single-phase thin film [10,11,12,13]. Multilayer is the most conventional approach to obtain the EB effect, which alternatively grows FM and AFM layers to create a transverse FM/AFM interface. The multilayers could be stacked by different material combinations, such as metal/alloy, metal/oxide and oxide/oxide, for example. Co/CuMn bilayer, Fe/FeO bilayer and La0.7Sr0.3MnO3 (LSMO)/BiFeO3 (BFO) bilayer have been designed to investigate their EB effect [14,15,16]. The HEB could be tailored by tuning the number of layer and the thickness of each layer, for example, the relationship between HEB and the thickness of the FM layer (tFM) is derived as HEB ∝ 1/tFM [17]. The composite thin film evolving FM and AFM components is another platform to achieve EB, which forms a unique nanostructure of one phase exhibited as nanopillars embedding into another matrix phase, termed as vertically aligned nanocomposite (VAN) thin film. Different from the transverse FM/AFM interface in multilayers, VAN thin film presents FM/AFM coupling along the vertical direction, which is beneficial to realize perpendicular EB effect. Various oxide systems have been explored, such as LSMO:NiO, LSMO:LaFeO3 (LFO), NiO:NiFe2O4 (NFO), BFO:Fe3O4, etc. [18,19,20,21,22]. Similar lattice parameters/crystal structures and phase immiscibility are required to form such VAN structure, otherwise it is highly possible to be phase mixed as a solid solution or composite thin film. Solid solution thin films with FM and AFM phases can also induce the EB effect by the FM/AFM exchange coupling in nanoscale interface [12]. Lastly, the EB effect has been observed even in single-phase thin films, which is induced by either defects [23], strain [24] or some unusual interfaces [13,25]. Overall, although the EB effect has been obtained in variety of thin films with different nanostructures, there are still plenty of material systems and geometries needing further investigation.
In this work, a new FM-AFM system has been developed for the EB effect, e.g., LFO and La0.7Ca0.3MnO3 (LCMO) are selected as the AFM phase and FM phase, respectively. We deposited LFOx:LCMO1−x (x = 0.33, 0.5, 0.67) composite thin films by pulsed laser deposition (PLD) and investigated their EB effect; the thickness of the films was controlled at ~200 nm. Both LFO (a = 3.940 Å, pseudo-cubic) and LCMO (a = 3.867 Å, pseudo-cubic) present perovskite structures with lattice parameters close to the selected STO (001) substrate (a = 3.905 Å, cubic). LFO is a typical AFM material (TN = 710 K) and has been applied in various systems with an EB effect [19,26,27], while LCMO is a widely studied FM material (Curie temperature TC = 225 K). [28] Therefore, the EB effect is expected in the LFO:LCMO composite thin film, and the HEB value can be tailored by varying the composition of the two phases.

2. Materials and Methods

Target Preparation and Thin Film Deposition: LFOx:LCMO1−x (x = 0.33, 0.5, 0.67) targets were made by a conventional solid-state mixing of the LFO and LCMO powders with the designed ratio, high-pressure pressing into a 1-inch pellet and followed by a sintering process at 1200 °C for 10 h. Then, the thin films were deposited using a pulsed laser deposition (PLD) system with a KrF excimer laser (Lambda Physik, λ = 248 nm). The detailed deposition parameters are as follows: base pressure was below 1 × 10−6 Torr, 45 Pa of high-purity O2 was inflowed into the chamber during deposition, the deposition temperature was 750 °C, the deposition frequency was 5 Hz, target-substrate distance was 4.5 cm and laser energy was 1 mJ/cm2; after deposition, 30 kPa O2 was inflowed into the chamber and the samples were cooled down at 10 °C/min.
Microstructure Characterizations: The crystal structure of the films was characterized by X-ray diffraction (XRD) (Panalytical X’Pert X-ray diffractometer). The surface morphology of the films was characterized by atomic force microscopy (AFM, Bruker Icon AFM).
Physical Property Characterizations: Temperature dependence of ZFC and FC magnetization (M-T, 5-380 K) and magnetic hysteresis curves (M-H, field along the direction perpendicular to the film surface) were carried out by using a vibrating sample magnetometer (VSM) in the physical property measurement system (PPMS: Quantum Design).

3. Results and Discussion

The main aspect of this work is to grow a new FM-AFM system with a tunable EB effect by composition variation of the two phases. First, standard θ–2θ XRD scans were characterized on the LFO:LCMO thin films with different compositions, as shown in Figure 1a–c for LFO0.33LCMO0.67, LFO0.5LCMO0.5 and LFO0.67LCMO0.33, respectively. Only LFO (00l) and LCMO (00l) peaks can be observed, which indicates the textured growth of both phases and that no impurity is formed in the composite films (note that the peak at ~42° is from the instrument, not from the samples). To obtain the actual 2θ values of the LFO (002) and LCMO (002) peaks, the local area (45–48°) has been enlarged and shown in the right panels of Figure 1. The 2θ values of the LFO (002) and LCMO (002) peaks can be identified as 46.285° and 46.607°, which corresponds to the d(001) values of 3.921 Å and 3.895 Å for LFO and LCMO, respectively. Compared to the bulk values, the LFO phase and LCMO phases in the composite thin film undergo out-of-plane compressive strain of −0.48% and tensile strain of 0.72%, respectively.
An atomic force microscope (AFM) has been used to investigate the surface morphology of the composite thin films, and the AFM images with 2 µm × 2 µm squares are shown in Figure 2a–c for LFO0.33LCMO0.67, LFO0.5LCMO0.5 and LFO0.67LCMO0.33 composite thin films, respectively. As is shown, LFO0.33LCMO0.67 presents a relatively rough surface with large domains, and the surface roughness (Ra) was determine to be 4.97 nm. On another side, LFO0.5LCMO0.5 and LFO0.67LCMO0.33 films exhibit a very smooth surface with Ra of 0.554 nm and 0.793 nm, and the domains are relatively small. It is highly possible that the neighboring domains are the FM and AFM phases; thus, the FM/AFM interfacial coupling occurs at the domain boundaries.
Then, the magnetization hysteresis (M-H) loops of all the samples were measured at different temperatures (10 K, 50 K, 150 K, 250 K and 300 K). The M-H loops of the LFO0.67LCMO0.33 film are shown in Figure 3a–d for 10 K, 50 K, 150 K and 250 K measurements; all of the loops exhibit typical M-H curves for hard magnets. An obvious EB effect can be identified, as a difference has been observed between the positive and negative coercivity. Another interesting feature is that the M-H curves are not smoothly presented; multiple steps can be observed, especially close to the saturation point that might result from the multiple magnetic components in the system, such as the FM LCMO phase, AFM LFO phase and the FM/AFM interface. The LFO0.33LCMO0.67 and LFO0.5LCMO0.5 samples exhibit similar shapes of the M-H loops with varying saturation magnetization (Ms) and coercivity (Hc) values (data not shown here).
Based on the M-H curves, the EB field (HEB = |H+ + H|/2), coercivity (HC = |H+ + H|/2 and Ms) values at different temperatures can be estimated and all the data for different samples are shown and compared in Figure 4a–c, respectively. When the temperature increases, the HEB and HC values decreases, which is a normal phenomenon in an AFM/FM system. Among the three samples with different composition, the LFO0.67LCMO0.33 film obtains the highest HEB and HC values at all the measured temperatures. The HEB values are 891 Oe, 459 Oe, 162 Oe and 28 Oe at 10 K, 50 K, 150 K and 250 K, respectively, and it diminishes at 300 K. The Ms values at different temperatures of all the samples are also compared in Figure 4c. The Ms values increase with a higher LCMO phase in the composite film as the FM LCMO has a much stronger magnetic response than the AFM LFO phase.
To further explore the magnetic properties of the composite thin film system, temperature dependence of zero-field cooling (ZFC) and field cooling (FC, 1000 Oe) magnetization (M-T) measurements of all the samples with different compositions have been carried out and compared in Figure 5. All the samples show a similar trend. For the FC condition, the magnetization decreases with increasing temperature (10−350 K) monotonically. However, for ZFC condition, magnetization firstly increases to a maximum value (blocking temperature: TB) and then decreases with increasing temperature. Another feature is the bifurcation between the ZFC and FC curves, which could be used to define the irreversibility temperature (Tirr). The TB value is slightly lower than Tirr, which has been observed in many other magnetic systems [29,30]. Overall, the LFO:LCMO composite thin films presents an interesting magnetic response; specifically, the large HEB values demonstrate a strong exchange interfacial coupling between the AFM LFO phase and FM LCMO phase. This new FM-AFM design provides more insights into how to develop composite thin films with the EB effect, and how to tune and optimize the HEB values via deposition condition optimization and composition variation to generate different nanostructures.

4. Conclusions

A new composite thin film system of LFO:LCMO with different compositions has been grown and characterized in order to achieve a tailorable exchange bias effect by composition variation. The composite thin films show excellent crystal quality with c-axis growth for both the LFO and LCMO phases. Furthermore, an obvious shift of the hysteresis loops has been observed for all the films, while the LFO0.67LCMO0.33 sample obtains the strongest FM-AFM interfacial exchange coupling. The HEB values of such film are estimated as 891 Oe, 459 Oe, 162 Oe and 28 Oe at 10 K, 50 K, 150 K and 250 K, respectively, which is relatively large compared to other oxide–oxide composite thin films. Furthermore, both blocking temperature and irreversibility temperature can be determined from the FC and ZFC M-T measurements.

Author Contributions

Conceptualization, C.J. and J.H.; methodology, F.W. and W.F.; formal analysis, F.W., W.F. and J.L.; investigation, F.W., W.F. and C.J.; resources, J.H.; writing—original draft preparation, F.W. and W.F.; writing—review and editing, C.J., J.L. and J.H.; supervision, J.H.; project administration, J.H.; funding acquisition, J.H. All authors have read and agreed to the published version of the manuscript.

Funding

J.H. acknowledges the support from Guangdong Basic and Applied Basic Research Foundation (2019A1515111029) and the Fundamental Research Funds for the Central Universities (20lgpy13). F.W acknowledges the support from Qing Lan project.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data is contained within the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Meiklejohn, W.H.; Bean, C.P. New magnetic anisotropy. Phys. Rev. 1956, 105, 904–913. [Google Scholar] [CrossRef]
  2. Wei, Z.; Sharma, A.; Nunez, A.S.; Haney, P.M.; Duine, R.A.; Bass, J.; MacDonald, A.H.; Tsoi, M. Changing exchange bias in spin valves with an electric current. Phys. Rev. Lett. 2007, 98, 116603. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  3. Klug, M.J.; Thormählen, L.; Röbisch, V.; Toxværd, S.D.; Höft, M.; Knöchel, R.; Quandt, E.; Meyners, D.; McCord, J. Antiparallel exchange biased multilayers for low magnetic noise magnetic field sensors. Appl. Phys. Lett. 2019, 114, 192410. [Google Scholar] [CrossRef]
  4. Tian, Z.; Xu, L.; Gao, Y.; Yuan, S.; Xia, Z. Magnetic memory effect at room temperature in exchange coupled NiFe2O4-NiO nanogranular system. Appl. Phys. Lett. 2017, 11, 182406. [Google Scholar] [CrossRef]
  5. Liao, X.; Gao, L.; Wang, Y.; Xu, X.; Khan, M.T.; Chang, T.; Chen, K.; Zeng, Y.; Yang, S.; Svedlindh, P. Large exchange bias in magnetic shape memory alloys by tuning magnetic ground state and magnetic-field history. Sci. China Mater. 2020, 63, 1291–1299. [Google Scholar] [CrossRef]
  6. Franceschin, G.; Gaudisson, T.; Menguy, N.; Dodrill, B.C.; Yaacoub, N.; Grenèche, J.; Valenzuela, R.; Ammar, S. Exchange-biased Fe3-xO4−CoO granular composites of different morphologies prepared by seed-mediated growth in polyol: From core-shell to multicore embedded structures. Part. Part. Syst. Charact. 2018, 35, 1800104. [Google Scholar] [CrossRef]
  7. Binns, C.; Qureshi, M.T.; Peddis, D.; Baker, S.H.; Howes, P.B.; Boatwright, A.; Cavill, S.A.; Dhesi, S.S.; Lari, L.; Kröger, R.; et al. Exchange bias in Fe@Cr core-shell nanoparticles. Nano Lett. 2013, 13, 3334–3339. [Google Scholar] [CrossRef] [Green Version]
  8. Sessi, V.; Hertenberger, S.; Zhang, J.; Schmitz, D.; Gsell, S.; Schreck, M.; Morel, R.; Brenac, A.; Honolka, J.; Kern, K. Exchange bias in reduced dimensions: Cobalt nanocluster arrays under the influence of nanometer thin MnPt capping layers. J. Appl. Phys. 2013, 113, 123903. [Google Scholar] [CrossRef]
  9. Blachowicz, T.; Ehrmann, A. Exchange bias in thin films-an update. Coatings 2021, 11, 122. [Google Scholar] [CrossRef]
  10. Maat, S.; Takano, K.; Parkin, S.S.P.; Fullerton, E.E. Perpendicular exchange bias of Co/Pt multilayers. Phys. Rev. Lett. 2001, 87, 087202. [Google Scholar] [CrossRef]
  11. Huang, J.; Gellatly, A.; Kauffmann, A.; Sun, X.; Wang, H. Exchange bias effect along vertical interfaces in La0.7Sr0.3MnO3:NiO vertically aligned nanocomposite thin films integrated on silicon substrates. Cryst. Growth Des. 2018, 18, 4388–4394. [Google Scholar] [CrossRef]
  12. Lorenz, M.; Ziese, M.; Wagner, G.; Lenzner, J.; Kranert, C.; Brachwitz, K.; Hochmuth, H.; Esquinazi, P.; Grundmanna, M. Exchange bias and magnetodielectric coupling effects in ZnFe2O4-BaTiO3 composite thin films. CrystEngComm 2012, 14, 6477–6486. [Google Scholar] [CrossRef]
  13. Sung, K.D.; Park, Y.A.; Seo, M.S.; Jo, Y.; Hur, N.; Jung, J.H. Observation of intriguing exchange bias in BiFeO3 thin films. J. Appl. Phys. 2012, 112, 033915. [Google Scholar] [CrossRef]
  14. Ali, M.; Adie, P.; Marrows, C.H.; Greig, D.; Hickey, B.J.; Stamps, R.L. Exchange bias using a spin glass. Nat. Mater. 2007, 6, 70–75. [Google Scholar] [CrossRef] [PubMed]
  15. Fan, Y.; Smith, K.J.; Lüpke, G.; Hanbicki, A.T.; Goswami, R.; Li, C.H.; Zhao, H.B.; Jonker, B.T. Exchange bias of the interface spin system at the Fe/MgO interface. Nat. Nanotechnol. 2013, 8, 438–444. [Google Scholar] [CrossRef]
  16. Wu, S.M.; Cybart, S.A.; Yu, P.; Rossell, M.D.; Zhang, J.X.; Ramesh, R.; Dynes, R.C. Reversible electric control of exchange bias in a multiferroic field-effect device. Nat. Mater. 2010, 9, 756–761. [Google Scholar] [CrossRef] [PubMed]
  17. Leighton, C.; Fitzsimmons, M.R.; Hoffmann, A.; Dura, J.; Majkrzak, C.F.; Lund, M.S.; Schuller, I.K. Thickness-dependent coercive mechanisms in exchange-biased bilayers. Phys. Rev. B 2002, 65, 064403. [Google Scholar] [CrossRef] [Green Version]
  18. Ning, X.; Wang, Z.; Zhang, Z. Large, temperature-tunable low-field magnetoresistance in La0.7Sr0.3MnO3:NiO nanocomposite films modulated by microstructures. Adv. Funct. Mater. 2014, 24, 5393–5401. [Google Scholar] [CrossRef]
  19. Fan, M.; Zhang, W.; Jian, J.; Huang, J.; Wang, H. Strong perpendicular exchange bias in epitaxial La0.7Sr0.3MnO3:LaFeO3 nanocomposite thin films. APL Mater. 2016, 4, 076105. [Google Scholar] [CrossRef] [Green Version]
  20. Huang, J.; Wang, H.; Wang, X.; Gao, X.; Liu, J.; Wang, H. Exchange bias in a La0.67Sr0.33MnO3/NiO heterointerface integrated on a flexible mica substrate. ACS Appl. Mater. Interfaces 2020, 12, 39920–39925. [Google Scholar] [CrossRef]
  21. Wu, R.; Yun, C.; Wang, X.; Lu, P.; Li, W.; Lin, Y.; Choi, E.; Wang, H.; MacManus-Driscoll, J.L. All-oxide nanocomposites to yield large, tunable perpendicular exchange bias above room temperature. ACS Appl. Mater. Interfaces 2018, 10, 42593–42602. [Google Scholar] [CrossRef]
  22. Choi, E.; Weal, E.; Bi, Z.; Wang, H.; Kursumovic, A.; Fix, T.; Blamire, M.G.; MacManus-Driscoll, J.L. Strong room temperature exchange bias in self-assembled BiFeO3-Fe3O4 nanocomposite heteroepitaxial films. Appl. Phys. Lett. 2013, 102, 012905. [Google Scholar] [CrossRef]
  23. Wang, C.; Chen, C.; Chang, C.; Tsai, H.; Pandey, P.; Xu, C.; Böttger, R.; Chen, D.; Zeng, Y.; Gao, X.; et al. Defect-induced exchange bias in a single SrRuO3 layer. ACS Appl. Mater. Interfaces 2018, 10, 27472–27476. [Google Scholar] [CrossRef] [Green Version]
  24. Zhou, G.; Ji, H.; Bai, Y.; Quan, Z.; Xu, X. Intrinsic exchange bias effect in strain-engineered single antiferromagnetic LaMnO3 films. Sci. China Mater. 2019, 62, 1046–1052. [Google Scholar] [CrossRef] [Green Version]
  25. West, K.G.; Nam, D.N.H.; Lu, J.W.; Bassim, N.D.; Picard, Y.N.; Stroud, R.M.; Wolf, S.A. Exchange bias in a single phase ferrimagnet. J. Appl. Phys. 2010, 107, 113915. [Google Scholar] [CrossRef]
  26. Scholl, A. Domain-size-dependent exchange bias in Co/LaFeO3. Appl. Phys. Lett. 2004, 85, 4085. [Google Scholar] [CrossRef] [Green Version]
  27. Mohamed, A.A.; Álvarez-Alonso, P.; Hernando, B. The intrinsic exchange bias effect in the LaMnO3 and LaFeO3 compounds. J. Alloys Compd. 2021, 850, 156713. [Google Scholar] [CrossRef]
  28. Nurgaliev, T.; Topal, U.; Blagoev, B.; Mateev, E. Magnetic properties of LCMO/LSMO thin films on LAO and ALO substrates. J. Supercond. Nov. Magn. 2012, 25, 2495–2498. [Google Scholar] [CrossRef]
  29. Alonso, J.; Fdez-Gubieda, M.L.; Barandiarán, J.M.; Svalov, A.; Fernández Barquín, L.; Venero, D.A.; Orue, I. Crossover from superspin glass to superferromagnet in FexAg100-x nanostructured thin films (20 ≤ x ≤ 50). Phys. Rev. B 2010, 82, 054406. [Google Scholar] [CrossRef]
  30. Huang, X.H.; Ding, J.F.; Jiang, Z.L.; Yin, Y.W.; Yu, Q.X.; Li, X.G. Dynamic properties of cluster glass in La0.25Ca0.75MnO3 nanoparticles. J. Appl. Phys. 2009, 106, 083904. [Google Scholar] [CrossRef]
Figure 1. Standard θ–2θ XRD scans on LFO:LCMO thin films with different compositions. (a) LFO0.33LCMO0.67; (b) LFO0.5LCMO0.5 and (c) LFO0.67LCMO0.33. The right panels are the local scan from 45° to 48°.
Figure 1. Standard θ–2θ XRD scans on LFO:LCMO thin films with different compositions. (a) LFO0.33LCMO0.67; (b) LFO0.5LCMO0.5 and (c) LFO0.67LCMO0.33. The right panels are the local scan from 45° to 48°.
Coatings 11 01125 g001
Figure 2. Atomic force microscopic images to show the surface morphology of (a) LFO0.33LCMO0.67, (b) LFO0.5LCMO0.5 and (c) LFO0.67LCMO0.33 composite thin films.
Figure 2. Atomic force microscopic images to show the surface morphology of (a) LFO0.33LCMO0.67, (b) LFO0.5LCMO0.5 and (c) LFO0.67LCMO0.33 composite thin films.
Coatings 11 01125 g002
Figure 3. The magnetization hysteresis (M-H) loops of the LFO0.67LCMO0.33 film measured at (a) 10 K, (b) 50 K, (c) 150 K and (d) 250 K.
Figure 3. The magnetization hysteresis (M-H) loops of the LFO0.67LCMO0.33 film measured at (a) 10 K, (b) 50 K, (c) 150 K and (d) 250 K.
Coatings 11 01125 g003
Figure 4. Magnetic properties comparison of the composite thin films with different compositions, which are (a) HEB value, (b) HC value and (c) Ms value.
Figure 4. Magnetic properties comparison of the composite thin films with different compositions, which are (a) HEB value, (b) HC value and (c) Ms value.
Coatings 11 01125 g004
Figure 5. Temperature dependence of zero-field cooling (ZFC, solid symbols) and field cooling (FC, 1000 Oe, hollow symbols) magnetization of all the samples with different compositions.
Figure 5. Temperature dependence of zero-field cooling (ZFC, solid symbols) and field cooling (FC, 1000 Oe, hollow symbols) magnetization of all the samples with different compositions.
Coatings 11 01125 g005
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Wang, F.; Fu, W.; Jiang, C.; Li, J.; Huang, J. Exchange Bias Effect in LaFeO3: La0.7Ca0.3MnO3 Composite Thin Films. Coatings 2021, 11, 1125. https://doi.org/10.3390/coatings11091125

AMA Style

Wang F, Fu W, Jiang C, Li J, Huang J. Exchange Bias Effect in LaFeO3: La0.7Ca0.3MnO3 Composite Thin Films. Coatings. 2021; 11(9):1125. https://doi.org/10.3390/coatings11091125

Chicago/Turabian Style

Wang, Feng, Wei Fu, Chengming Jiang, Junxiao Li, and Jijie Huang. 2021. "Exchange Bias Effect in LaFeO3: La0.7Ca0.3MnO3 Composite Thin Films" Coatings 11, no. 9: 1125. https://doi.org/10.3390/coatings11091125

APA Style

Wang, F., Fu, W., Jiang, C., Li, J., & Huang, J. (2021). Exchange Bias Effect in LaFeO3: La0.7Ca0.3MnO3 Composite Thin Films. Coatings, 11(9), 1125. https://doi.org/10.3390/coatings11091125

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.