Next Article in Journal
Using XGBoost Regression to Analyze the Importance of Input Features Applied to an Artificial Intelligence Model for the Biomass Gasification System
Next Article in Special Issue
Design and 3D Manufacturing of an Improved Heliostatic Illuminator
Previous Article in Journal / Special Issue
A New Mechanism of Male Plug for Electrical Protection
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Method of the Mechanical Properties Evaluation of Polyethylene Gas Pipelines with Portable Hardness Testers

by
Anna Vinogradova
1,
Kirill Gogolinskii
1,
Alexander Umanskii
1,*,
Varvara Alekhnovich
1,
Alena Tarasova
1 and
Alena Melnikova
2
1
Department of Metrology, Instrumentation and Quality Management, Saint Petersburg Mining University, 199106 Saint Petersburg, Russia
2
Department of Mineral Raw Materials Processing, Saint Petersburg Mining University, 199106 Saint Petersburg, Russia
*
Author to whom correspondence should be addressed.
Inventions 2022, 7(4), 125; https://doi.org/10.3390/inventions7040125
Submission received: 12 November 2022 / Revised: 6 December 2022 / Accepted: 8 December 2022 / Published: 13 December 2022
(This article belongs to the Collection Feature Innovation Papers)

Abstract

:
This article is devoted to the study of means and methods for non-destructive testing mechanical properties of polyethylene gas pipelines that have been in operation for 25–55 years. In order to assess mechanical properties, stress at yield was chosen as a key parameter. Stress at yield is determined from the results of tensile tests and is associated with the limiting circumferential (hoop) stress, determined from the results of tests for short-term pressure. Tensile tests require sample cutting and the shutdown of pipelines’ service. To solve this problem of nondestructive testing of pipelines, tests were carried out using the methods of Shore, Leeb and dynamic instrumental indentation. According to the test results, it was revealed that the correlation coefficient between the values of stress at yield and hardness, obtained by the method of dynamic instrumental indentation, is 0.98 which confirms the possibility of the evaluation of the mechanical properties of pipelines by the method of dynamic instrumental indentation.

1. Introduction

Transportation of natural gas, oil and other liquid and gaseous products is carried out through pipelines of various types [1,2,3]. Polyethylene pipes are widely used for natural gas transportation in regional gas distribution systems. The construction of polyethylene (PE) gas pipelines was started more than 60 years ago, and the first PE gas pipelines in the Russian Federation were built more than 55 years ago. At present, their total length is more than 300 thousand km.
PE pipes have significant advantages over steel pipes when transporting gas. This applies to the ease of manufacturing and cost of pipeline construction, operational parameters, as well as reliability and durability [4,5,6]. PE pipes, unlike steel [7,8,9], are not exposed to internal and external corrosion. The world’s experience in the operation of PE gas pipelines has confirmed their high reliability in a variety of conditions [10,11,12], including the impact of catastrophic earthquakes [13].
At the same time, with all the reliability and durability of the gas pipelines, they are exposed to various degradation processes occurring under the influence of ultraviolet radiation [14,15], as well as aggressive environments [16,17,18]. The first factor is excluded by the fact that all PE gas pipelines are laid underground. The transported natural gas has a low content of aggressive chemical elements. In this regard, the main harmful effects on the pipe material are associated with the chemical composition of soils and groundwater, as well as mechanical deformations of the soil [19,20]. In addition, it is well-known that, over many years of service, PE pipes are exposed to long-term changes in the structure of thermoplastics, leading to an increase in the degree of crystallinity and, as a consequence, an increase in the rigidity and brittleness of the material [21,22,23]. External influences and internal processes lead to changes of the pipe material’s original properties over time.
Regulatory documents define the safe operation period of gas pipelines as 50 years. Currently, the length of gas pipelines that are older than 50 years in the Russian Federation amounts to tens of kilometers, but in the next decade this value will increase to tens of thousands kilometers. In this regard, the task of developing methods for technical diagnostics of gas pipelines with long service life and assessing their residual life is crucial [24,25].
Currently, there are a number of regulatory requirements for PE properties and pipes used for the construction of gas pipelines [26,27,28]. These requirements apply, among other things, to the physicochemical and mechanical properties. Determination of this parameters is carried out both on small-scale PE samples and on entire sections of pipes up to a meter in size or more. A common feature of all these requirements is that they apply to new pipes. Appropriate tests are carried out during the development of technological processes, as well as to confirm the quality of finished products. Currently, there are no regulatory documents to establish requirements and test methods for pipes that have been in long-term operation. The use of standard test procedure to assess mechanical properties of in-service pipelines has its flaws, such as:
  • Pipes that have been in operation for several decades do not meet modern requirements, which does not interfere with their safe operation;
  • The requirements for new pipes imply their resistance to various mechanical stresses during construction, while in-service pipelines do not experience such loads;
  • A complete list of tests of PE pipes implies the use of full-size samples, which, in the case of gas pipelines in operation, requires their complete shutdown in order to cut long sections of pipes (up to 10 m) with subsequent repair.
In summary, it is crucial to develop non-destructive methods for diagnosing the state of PE pipelines using small-scale samples. One of the key parameters characterizing the operational properties of a pipe is its mechanical properties, which provide resistance to internal gas pressure and strength under external influences [29]. In this research, the study of means and methods of non-destructive evaluation of PE pipes’ mechanical properties is presented.

2. Materials and Methods

2.1. Samples

PE pipe samples were cut from both operating gas pipelines with 25–55 years of service and a new pipeline. A detailed description of the samples, as well as the results of a study of their physicochemical properties, are presented in [30]. The list of selected samples and their characteristics are given in Table 1.

2.2. Standard Methods for Mechanical Testing of PE Pipes

The decrease in the performance of polymer pipes is characterized by the loss of the ability to resist plastic destruction and the occurrence of brittle fracture. Modern grades of polyethylene (for example, PE 100) had high long-term strength and a sufficient safety factor. Despite the development of safe and efficient materials for pipes of underground gas pipelines, diagnostics and monitoring of the condition of such gas pipelines are a very important task, especially the study of the mechanical properties of materials under conditions similar to operational conditions.
PE pipes’ characteristics are fixed by the ISO 4437-1, where the main group is mechanical properties [26], such as:
  • resistance to internal pressure [31];
  • elongation at break [32];
  • resistance to slow crack propagation [33];
  • resistance to rapid crack propagation [34].
Tests to determine the resistance to internal pressure according to ISO 1167-1 [31] are used to assess the properties and service life of PE pipelines, their short-term and long-term strength characteristics. The result of a long-term pressure test suggests the presence of a transition point from ductile to brittle fracture along the time of thermal action [35].
Tensile tests are used to characterize the mechanical properties of a polymer in terms of modulus of elasticity, strength and elongation at break. The elongation at break is determined according to ISO 6259-1 [32] in tensile tests using a tensile testing machine.
An important indicator that determines the service life of PE gas pipelines is the ability of the material to resist crack propagation. During the processes of transportation, storage and installation, polyethylene pipes are at risk of damage. The characteristic of resistance to slow crack propagation determines the process of destruction of the material in the presence of a stress concentrator in the form of an initial defect. Resistance to rapid crack propagation characterizes the resistance of a pipe to point mechanical impacts with large stress gradients.
The considered standard methods for diagnosing the mechanical characteristics of gas pipelines involve testing of full-size samples. In this case, it becomes necessary to suspend the operation of the gas pipeline for a long time, which causes economic losses. Full-scale standard tests do not allow of assessing changes in the mechanical properties of PE pipes over time [36]. Therefore, it is proposed to consider the possibility of using small-scale tests to study the mechanical properties.

2.3. Non-Destructive Test Methods

Hardness measurement methods are the most common non-destructive tests to evaluate the mechanical properties of materials. Hardness measurements are often used to study the mechanical properties of polymers [37]. Since hardness testers are used in laboratory conditions (Brinell, Vickers, Rockwell) they are inapplicable for solving the tasks set, so portable hardness testers were chosen for the study [38]. In order to select the most suitable method for measuring hardness, tests were carried out using portable hardness testers of various hardness scales: Shore; Leeb and the dynamic instrumental indentation.
Shore hardness is the most commonly used method for testing the hardness of plastics. The standard [39] specifies a method for determining the hardness of plastics and ebonite by static indentation using two types of durometers: the type A durometer, used for testing softer plastics; and the type D durometer, for testing harder plastics. The Shore method is an empirical test designed primarily for quality control of plastics. To measure the hardness of samples by the Shore method, a hardness tester “NDTone TS” of type D was used [40].
The method of measuring hardness using Leeb scales is based on determining the ratio of the velocities of the impact body during the rebound and impact phases of the indentation process [41]. This method belongs to the dynamic methods of hardness measurements. Leeb hardness testers are widely used for technical diagnostics of the condition of various parts and structures [42,43,44].
A NDTone KT-C hardness tester with a Type C transducer were used to carry out measurements in this work, since it has the lowest impact energy of all standardized types of Leeb transducers [41,45].
The method of dynamic instrumental indentation (DII) [46] and its application to determine various mechanical properties of materials are considered in detail in [47]. There are works in which the DII method was used to study the elastoplastic properties of polymers [48,49].
In the present study, we used a device that implements the DII method similar to that described in [50]. Measurements were taken with a spherical indenter of 1.5-mm diameter and impact energy of 1.9 mJ.

3. Results

The stress at yield σy, determined from the results of tensile tests according to ISO 527-2 [51], was chosen as the main parameter characterizing the mechanical properties of PE. Type 1B test specimens were cut from each sample. Table 2 shows the average values of the test results for five test specimens for each pipe, as well as the calculated standard deviation (SD).
As part of the study, tests for short term pressure in accordance with ISO 4437-3 [28] were also carried out. The results of the pressure at failure Pp were obtained, which were then recalculated into the limiting circumferential (hoop) stress in the pipe wall σc (Table 2) according to the equation:
σ c = P p d e m e m i n e m i n
where Pp—pressure at failure, MPa; dem—outer diameter of the pipe, mm; emin—minimum measured pipe wall thickness, mm. This test was carried out once for each sample, since it requires a significant length of pipe. The type of fracture was also recorded; all samples were plastically fractured.
Tests according to the Shore, Leeb and DII methods were carried out directly on pipes without preliminary sample preparation. Several series of measurements were taken at five points on the surface of each pipe. The average value and corresponding standard deviation of hardness values are given in Table 2.
The results obtained from the experiment were analyzed:
an assessment was made of the correspondence between the stress at yield, determined by tensile tests and limiting circumferential (hoop) stress, determined by the short-term pressure tests of full-size samples;
the results of hardness measurements and stress at yield were compared by the value of standard deviation;
the correlation coefficients between the values of hardness and stress at yield are calculated.
Comparison of the values of the stress at yield and limiting circumferential (hoop) stress is shown in the Figure 1. The standard deviation of the stress at yield values for different samples does not exceed 2% of the average value, which makes it possible to use it as a reference value. There is a good correlation between the result of a standard mechanical tensile test and the value of the limiting circumferential (hoop) stress, which characterizes the mechanical strength of the pipe under operating conditions. The limiting circumferential (hoop) stress in this experiment exceeds the stress at yield on average by 10%.
The results of hardness measurements are shown in Figure 2. Comparison of the dispersion of hardness measurements by different methods demonstrates the obvious advantage of the DII method. The values of the correlation coefficient between the values of the stress at yield and the hardness values according to the methods of Shore, Leeb and DII were 80%, 82% and 98%, respectively. Thus, it was concluded that the DII method is the most preferable for determining the yield stress of PE by a non-destructive methods.
To analyze the possibility of converting the hardness values according to the DII method (HDII) into the values of the stress at yield (σy) the coefficient K was proposed. The K coefficient value is equal to the ratio of the stress at yield σy to the hardness values HDII (Table 3). The sample from 1978 may be excluded from the analysis due to the large deviation of its properties from other samples. In that case, the average value of the K coefficient is 0.14, while the maximum deviation does not exceed 7%.
The method for measuring the stress at yield by the DII method should include the calibration of the hardness tester by determining the coefficient K, which is equal to the ratio of the yield strength σy to the hardness value HDII, measured on one reference sample of the pipe. A new pipe can be taken as a reference sample, which eliminates the need to cut samples from existing pipelines

4. Discussion

The results obtained during this work made it possible to draw the following conclusions:
  • The values of stress at yield obtained during the tensile tests correlate well with the value of critical stress in the pipe wall determined during the short-term pressure tests;
  • The method of DII demonstrates the best results in comparison with Shore and Leeb hardness testers, both in terms of the spread of measurement results (random error) and in terms of correlation with the values of the stress at yield determined from the results of tensile tests;
  • The use of the DII method makes it possible to determine the stress at yield of the pipe material with high accuracy without cutting samples and stopping the operation of the gas pipeline.

5. Conclusions

The fact of a linear relationship between the yield stress and hardness of metals for static methods of measuring hardness is widely known. A similar relationship for thermoplastics has been much less studied. Measurements with a standard Shore hardness tester showed unsatisfactory results due to the large dispersion. Hardness values measured by dynamic methods (Leeb method) depend on the ratio of yield stress and modulus of elasticity. At the same time, the dynamic instrumental indentation method makes it possible to separately measure the elastic and plastic components of deformation, which determines its advantages over other methods. The study shows that the use of the DII method for evaluation of mechanical properties of polyethylene pipelines makes it possible to obtain results that have a slight random scatter and a high degree of correlation with the values of the stress at yield determined by tensile tests and limiting circumferential (hoop) stress, determined during the short-term pressure tests. The stress at yield of PE pipes of various grades and ages can be measured by the DII method by properly calibrating the instrument on a sample of PE pipe with a known value of stress at yield. Thus, the DII method can be effectively used for non-destructive testing of the technical condition of polyethylene pipelines in operation.

Author Contributions

Conceptualization, K.G.; Methodology, K.G.; Validation, V.A., A.T. and A.M.; Formal analysis, A.V. and A.U.; Resources, V.A. and A.T.; Data curation, A.V. and A.U.; Writing—original draft, A.U. and K.G.; Writing—review & editing, K.G. and A.U.; Visualization, A.M.; Project administration, K.G. All authors have read and agreed to the published version of the manuscript.

Funding

The study was carried out as part of research work on the basis of agreement No. Upr6-026/20 dated 12 February 2020 with Gazprom Gazoraspredelenie JSC.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Acknowledgments

The authors would like to thank Dmitry Sergeevich Gromyka, a post-graduate student of Saint-Petersburg Mining University, for his assistance in conducting tensile tests, as well as to the testing center of the Klimovsky Pipe Plant for conducting short-term pressure tests.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Carranza, J.R.Z.; Kovshov, S.; Lyubin, E. Assessment of anthropogenic factor of accident risk on the main oil pipeline pascuales-cuenca in Ecuador. J. Appl. Eng. Sci. 2018, 16, 307–312. [Google Scholar] [CrossRef]
  2. Bakesheva, A.E. Determination of natural gas loss values based on physical simulation of leakages from the pipeline to the media with superatmospheric pressure using a volumetric-type expander. News Natl. Acad. Sci. Repub. Kazakhstan Ser. Geol. Tech. Sci. 2019, 3, 114–121. [Google Scholar] [CrossRef]
  3. Voronov, V.A. Peculiarities of flow of liquefied natural gas in pipelines. In Youth Technical Sessions Proceedings, Proceedings of the 6th Youth Forum of the World Petroleum Council- Future Leaders Forum, Saint Petersburg, Russia, 23–28 June 2019; CRC Press: Boca Raton, FL, USA, 2019; pp. 126–132. [Google Scholar] [CrossRef]
  4. Frank, A.; Pinter, G.; Lang, R.W. Prediction of the remaining lifetime of polyethylene pipes after up to 30 years in use. Polym. Test. 2009, 28, 737–745. [Google Scholar] [CrossRef]
  5. Wang, Y.; Lan, H.; Meng, T. Lifetime prediction of natural gas polyethylene pipes with internal pressures. Eng. Fail. Anal. 2019, 5, 154–163. [Google Scholar] [CrossRef]
  6. Bachir-Bey, T.; Belhaneche-Bensemra, N. Investigation of Polyethylene Pipeline Behavior after 30 Years of Use in Gas Distribution Network. J. Mater. Eng. Perform. 2020, 29, 6652–6660. [Google Scholar] [CrossRef]
  7. Goldobina, L.A.; Orlov, P.S. Analysis of the corrosion destruction causes in underground pipelines and new solutions for increasing corrosion steel’s resistance. J. Min. Inst. 2016, 219, 459. [Google Scholar] [CrossRef]
  8. Ivanik, S.A. Chemical and electrochemical methods of protection from corrosion of gas and oil pipelines and storage tanks. Int. Multidiscip. Sci. GeoConf. Surv. Geol. Min. Ecol. Manag. SGEM 2017, 17, 579–584. [Google Scholar] [CrossRef]
  9. Bakesheva, A.T. A refined algorithm for leak location in gas pipelines with determination of quantitative parameters. Int. J. Eng. Res. Technol. 2019, 12, 2867–2869. [Google Scholar]
  10. Chaoui, K.; Khelif, R.; Zeghib, N.; Chateauneuf, A. Failure Analysis of Polyethylene Gas Pipes. In Safety, Reliability and Risks Associated with Water, Oil and Gas Pipelines; Pluvinage, G., Elwany, M.H., Eds.; NATO Science for Peace and Security Series; Springer: Dordrecht, The Netherlands, 2008. [Google Scholar] [CrossRef]
  11. Majid, F.; Rhanim, R.; Lahlou, M.; Rhanim, H.; Ezzahi, M.; Elghorba, M. Maintainability and reliability of high density polyethylene pipes through experimental and theoretical models. Procedia Struct. Integr. 2020, 5, 430–437. [Google Scholar] [CrossRef]
  12. Lyubchik, A.N.; Krapivskii, E.I.; Bol’shunova, O.M. Prediction of the technical status of pipeline based on analysis. J. Min. Inst. 2011, 192, 153. [Google Scholar]
  13. Hideki, O.; Tomokazu, H. Polyethylene Pipeline Performance against Earthquake. In Proceedings of the 19th Plastic Pipes Conference PP XIX, Las Vegas, NV, USA, 24–26 September 2018. [Google Scholar]
  14. Gong, Y.; Wang, S.; Zhang, Z.; Yang, X.; Yang, Z.; Yang, H. Degradation of sunlight exposure on the high-density polyethylene (HDPE) pipes for transportation of natural gases. Polym. Degrad. Stab. 2021, 194, 109752. [Google Scholar] [CrossRef]
  15. Becerra, A.F.C.; d’Almeida, J.R.M. UV Effects on the Tensile and Creep Behaviour of HDPE. Polym. Polym. Compos. 2018, 25, 327–332. [Google Scholar] [CrossRef]
  16. Guo, S.-M.; Yang, Z.-G.; Tang, X.-Y.; Zuo, Y.-T. Safety assessment of high density polyethylene pipe with thermal damages. Plast. Rubber Compos. 2017, 46, 173–183. [Google Scholar] [CrossRef]
  17. Byrne, N.; Silva, R.; de Hilditch, T. Linking Antioxidant Depletion with Material Properties for Polyethylene Pipes Resins. Polym. Eng. Sci. 2020, 60, 323–329. [Google Scholar] [CrossRef]
  18. Norman, S.A.; Simon, J.P.; Marshal, G.P.; Jean, L.G. Environmental oxidation processes in yellow gas pipe: Implications for electrowelding. Polym. Degrad. Stab. 1997, 56, 265–274. [Google Scholar] [CrossRef]
  19. Bazhanova, M.E.; Svetlov, D.A.; Saltanova, T.A.; Grigorkina, O.P. Biological resistance of polymeric pipeline materials. IOP Conf. Ser. Mater. Sci. Eng. 2020, 3, 032036. [Google Scholar] [CrossRef]
  20. Choi, B.; Zhou, Z.; Chudnovsky, A.; Stivala, S.S.; Sehanobish, K.; Bosnyak, C.P. Fracture initiation associated with chemical degradation: Observation and modeling. Int. J. Solids Struct. 2005, 42, 681–695. [Google Scholar] [CrossRef]
  21. Khelif, R.; Chateauneuf, A.; Chaoui, K. Reliability-based assessment of polyethylene pipe creep lifetime. Int. J. Press. Vessel. Pip. 2007, 84, 697–707. [Google Scholar] [CrossRef]
  22. Weon, J. Effects of thermal ageing on mechanical and thermal behaviors of linear low density polyethylene pipe. Polym. Degrad. Stab. 2010, 95, 14–20. [Google Scholar] [CrossRef]
  23. Hubert, L.; David, L.; Séguéla, R.; Vigier, G.; Degoule, C.; Germain, Y. Physical and mechanical properties of polyethylene for pipes in relation to molecular architecture. I. Microstructure and crystallisation kinetics. Polymer 2001, 42, 8425–8434. [Google Scholar] [CrossRef]
  24. Proskuryakov, R.M.; Dement’ev, A.S. The building a system of diagnosing the technical condition of the pipeline on the basis of continuous pulsed magnetic field. J. Min. Inst. 2016, 218, 215. [Google Scholar]
  25. Yamilev, M.Z.; Pshenin, V.V.; Matveev, D.S.; Podlesniy, D.S.; Bezimyannikov, T.I. The use of compact inspection devices for monitoring the technical condition of pipelines in protective cases. Neft. Khozyaystvo- Oil Ind. 2022, 2, 106–110. [Google Scholar] [CrossRef]
  26. ISO 4437-1; Plastics Piping Systems for the Supply of Gaseous Fuels—Polyethylene (PE)—Part 1: General. ISO: Geneva, Switzerland, 2014.
  27. ISO 4437-2; Plastics Piping Systems for the Supply of Gaseous Fuels—Polyethylene (PE)—Part 2: Pipes. ISO: Geneva, Switzerland, 2014.
  28. ISO 4437-3; Plastics Piping Systems for the Supply of Gaseous Fuels—Polyethylene (PE)—Part 3: Fittings. ISO: Geneva, Switzerland, 2014.
  29. Baktizin, R.; Zaripov, R.; Korobkov, G.; Masalimov, R. Assessment of internal pressure effect, causing additional bending of the pipeline. J. Min. Inst. 2020, 242, 160. [Google Scholar] [CrossRef]
  30. Gogolinskiy, K.V.; Vinogradova, A.A.; Kopylova, T.N.; Povarov, V.G.; Vasilev, E.A.; Shchiptsova, E.K.; Rybkin, D.E.; Kolobov, D.S. Study of physicochemical properties of polyethylene gas pipelines material with a prolonged service life. Int. J. Press. Vessel. Pip. 2022, 200, 104825. [Google Scholar] [CrossRef]
  31. ISO 1167-1; Thermoplastics Pipes, Fittings and Assemblies for the Conveyance of Fluids—Determination of the Resistance to Internal Pressure—Part 1: General Method. ISO: Geneva, Switzerland, 2006.
  32. ISO 6259-1; Thermoplastics Pipes—Determination of Tensile Properties—Part 1: General Test Method. ISO: Geneva, Switzerland, 2015.
  33. ISO 13479; Polyolefin Pipes for the Conveyance of Fluids—Determination of Resistance to Crack Propagation—Test Method for Slow Crack Growth on Notched Pipes. ISO: Geneva, Switzerland, 2022.
  34. ISO 13477; Thermoplastics Pipes for the Conveyance of Fluids—Determination of Resistance to Rapid Crack Propagation (RCP)—Small-Scale Steady-State Test (S4 Test). ISO: Geneva, Switzerland, 2008.
  35. Bredács, M.; Frank, A.; Bastero, A.; Stolarz, A.; Pinter, G. Accelerated aging of polyethylene pipe grades in aqueous chlorine dioxide at constant concentration. Polym. Degrad. Stab. 2018, 157, 80–89. [Google Scholar] [CrossRef]
  36. Silva, R.; Hilditch, T.; Byrne, N. Assessing the integrity of in service polyethylene pipes. Polym. Test. 2018, 67, 228–233. [Google Scholar] [CrossRef]
  37. Briscoe, B.J.; Sinha, S.K. Hardness and Normal Indentation of Polymers. In Mechanical Properties and Testing of Polymers; Swallowe, G.M., Ed.; Springer: Dordrecht, The Netherlands, 1999; Volume 3, pp. 113–122. [Google Scholar] [CrossRef]
  38. Gogolinskii, K.V.; Syasko, V.A.; Umanskii, A.S.; Nikazov, A.A.; Bobkova, T.I. Mechanical properties measurements with portable hardness testers: Advantages, limitations, prospects. J. Phys. Conf. Ser. 2019, 1384, 012012. [Google Scholar] [CrossRef]
  39. ISO 868; Plastics and Ebonite—Determination of Indentation Hardness by Means of a Durometer (Shore Hardness). ISO: Geneva, Switzerland, 2003.
  40. Constanta. Available online: https://constanta.ru/catalog/tverdomery/konstanta_tsh/ (accessed on 10 November 2022).
  41. ISO 16859-1; Metallic Materials-Leeb Hardness Test—Part 1: Test Method. ISO: Geneva, Switzerland, 2015.
  42. Formisano, A.; Chiumiento, G.; Lorenzo, G.D. Leeb hardness experimental tests on carpentry steels: Surface treatment effect and empirical correlation with strength. AIP Conf. Proc. 2018, 1978, 450004. [Google Scholar] [CrossRef]
  43. Gromyka, D.S.; Gogolinskiy, K.V. Method of State and Residual Resource Assessment of Excavator Bucket Tooth Caps. Russ. J. Nondestruct. Test. 2022, 58, 381–390. [Google Scholar] [CrossRef]
  44. Liu, D.; Liu, X.; Fu, F. Nondestructive Post-fire Damage Assessment of Structural Steel Members Using Leeb Harness Method. Fire Technol. 2020, 56, 1777–1799. [Google Scholar] [CrossRef] [Green Version]
  45. DT1 KRAFT s.r.o. Available online: https://ndtone.com/product/kt-c-3/ (accessed on 11 November 2022).
  46. Rudnitsky, V.A.; Djakovicht, V.V. Material Testing by the Method of Dynamic Indentation. Nondestruct. Test. Eval. 1996, 12, 253–261. [Google Scholar] [CrossRef]
  47. Umanskii, A.; Gogolinskii, K.; Syasko, V.; Golev, A. Modification of the Leeb Impact Device for Measuring Hardness by the Dynamic Instrumented Indentation Method. Inventions 2022, 7, 29. [Google Scholar] [CrossRef]
  48. Vriend, N.M.; Kren, A.P. Determination of the viscoelastic properties of elastomeric materials by the dynamic indentation method. Polym. Test. 2004, 23, 369–375. [Google Scholar] [CrossRef]
  49. Martínez, A.B.; Arencón, D.; Navas, J.; Velasco, J.I. Low energy impact indentation of a modified polyethylene terephtalate by instrumented falling weight. J. Appl. Polym. Sci. 2013, 127, 2983–2989. [Google Scholar] [CrossRef]
  50. Pratasenia, T.A.; Kren, A.P.; Dyakova, H.N. Application of the Dynamic Indentation Method for Evaluation of the Hardness and Elastic Modulus of the Material of Products Obtained by Extrusion Method of Additive Production from Carbon-Filled Composite Materials. Mech. Compos. Mater. 2022, 58, 383–394. [Google Scholar] [CrossRef]
  51. ISO 527-2; Plastics—Determination of Tensile Properties—Part 2: Test Conditions for Molding and Extrusion Plastics. ISO: Geneva, Switzerland, 2012.
Figure 1. Results of mechanical tests.
Figure 1. Results of mechanical tests.
Inventions 07 00125 g001
Figure 2. (a) Shore hardness test results; (b) Leeb C hardness test results; (c) DII hardness test results.
Figure 2. (a) Shore hardness test results; (b) Leeb C hardness test results; (c) DII hardness test results.
Inventions 07 00125 g002
Table 1. Samples and their characteristics.
Table 1. Samples and their characteristics.
Year of ConstructionService Life, YearsDiameter, mmWall Thickness, mm
1965 5511010.0
1972481609.1
1978 4211011.8
1982 3811010.0
1989 3111010.0
1996 2411011.0
2020011010.1
Table 2. Results of tests and measurements of PE pipes.
Table 2. Results of tests and measurements of PE pipes.
SampleService Life, YearsShort-Term Pressure TestTensile TestsHardness Measurements
ShoreLeebDII
Limiting Circumferential (Hoop) Stress, σc, MPa,Stress at Yield, σy, MPaSD, %HSSD, %HLCSD, %HDIISD, %
20024.223.21.7731.86330.71632.2
962418.717.31.7663.26160.91356.7
893124.020.81.0713.86241.31493.3
823825.423.80.4694.56180.61571.8
784210.620.01.1565.55712.1894.5
724827.123.50.4643.96070.81683.0
655525.522.11.8723.16290.41641.2
Table 3. Values of K coefficient.
Table 3. Values of K coefficient.
SampleYears in Serviceσy, MPaHDIIK = σy/HDII
200231630.14
9624171350.13
8931211490.14
8238241570.15
78429890.10
7248241680.14
6555221640.13
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Vinogradova, A.; Gogolinskii, K.; Umanskii, A.; Alekhnovich, V.; Tarasova, A.; Melnikova, A. Method of the Mechanical Properties Evaluation of Polyethylene Gas Pipelines with Portable Hardness Testers. Inventions 2022, 7, 125. https://doi.org/10.3390/inventions7040125

AMA Style

Vinogradova A, Gogolinskii K, Umanskii A, Alekhnovich V, Tarasova A, Melnikova A. Method of the Mechanical Properties Evaluation of Polyethylene Gas Pipelines with Portable Hardness Testers. Inventions. 2022; 7(4):125. https://doi.org/10.3390/inventions7040125

Chicago/Turabian Style

Vinogradova, Anna, Kirill Gogolinskii, Alexander Umanskii, Varvara Alekhnovich, Alena Tarasova, and Alena Melnikova. 2022. "Method of the Mechanical Properties Evaluation of Polyethylene Gas Pipelines with Portable Hardness Testers" Inventions 7, no. 4: 125. https://doi.org/10.3390/inventions7040125

APA Style

Vinogradova, A., Gogolinskii, K., Umanskii, A., Alekhnovich, V., Tarasova, A., & Melnikova, A. (2022). Method of the Mechanical Properties Evaluation of Polyethylene Gas Pipelines with Portable Hardness Testers. Inventions, 7(4), 125. https://doi.org/10.3390/inventions7040125