Next Article in Journal
A New Way of Toughening of Thermoset by Dual-Cured Thermoplastic/Thermosetting Blend
Next Article in Special Issue
Fabrication of Nanopillar Crystalline ITO Thin Films with High Transmittance and IR Reflectance by RF Magnetron Sputtering
Previous Article in Journal
Systematic Investigation of the Synergistic and Antagonistic Effects on the Removal of Pyrene and Copper onto Mesoporous Silica from Aqueous Solutions
Previous Article in Special Issue
Nanostructure and Optical Property Investigations of SrTiO3 Films Deposited by Magnetron Sputtering
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Tailoring Electro/Optical Properties of Transparent Boron-Doped Carbon Nanowalls Grown on Quartz

1
Department of Materials, Environmental Sciences and Urban Planning, Università Politecnica delle Marche, 60131 Ancona, Italy
2
Department of Metrology and Optoelectronics, Faculty of Electronics, Telecommunication and Informatics, Gdańsk University of Technology, 80-233 Gdańsk, Poland
3
Polish Academy of Sciences, The Szewalski Institute of Fluid-Flow Machinery Fiszera 14, 80-231 Gdansk, Poland
4
Faculty of Applied Physics and Mathematics, Department of Solid State Physics, Gdansk University of Technology, 11/12 Narutowicza Str., 80-233 Gdansk, Poland
*
Authors to whom correspondence should be addressed.
Materials 2019, 12(3), 547; https://doi.org/10.3390/ma12030547
Submission received: 29 January 2019 / Revised: 8 February 2019 / Accepted: 10 February 2019 / Published: 12 February 2019
(This article belongs to the Special Issue Transparent Conductive Films and Their Applications)

Abstract

:
Carbon nanowalls (CNWs) have attracted much attention for numerous applications in electrical devices because of their peculiar structural characteristics. However, it is possible to set synthesis parameters to vary the electrical and optical properties of such CNWs. In this paper, we demonstrate the direct growth of highly transparent boron-doped nanowalls (B-CNWs) on optical grade fused quartz. The effect of growth temperature and boron doping on the behavior of boron-doped carbon nanowalls grown on quartz was studied in particular. Temperature and boron inclusion doping level allow for direct tuning of CNW morphology. It is possible to operate with both parameters to obtain a transparent and conductive film; however, boron doping is a preferred factor to maintain the transparency in the visible region, while a higher growth temperature is more effective to improve conductance. Light transmittance and electrical conductivity are mainly influenced by growth temperature and then by boron doping. Tailoring B-CNWs has important implications for potential applications of such electrically conductive transparent electrodes designed for energy conversion and storage devices.

Graphical Abstract

1. Introduction

Most commercial transparent electrodes are usually made of indium tin oxide (ITO) due to its good electrical performance (~10 Ω/square), while the limited amount of indium resources raises concerns in the European Union as well as globally. For this reason, the scientific community has moved to seek new solutions [1,2]; among those, carbon-based transparent conducting materials are extensively applied nowadays in many optoelectronic [3,4], biosensing [5,6], energy storage, and conversion devices [7,8,9]. Carbon nanostructures are particularly attractive due to their unique three-dimensional structure with a high surface area and specific surface interactions [10]. Alternative nanomaterials, such as carbon nanowalls (CNWs), have held the attention of the scientific community due to their structural characteristics in mono-, bi- and tri-dimensional arrangements [11,12,13], including excellent electrical and thermal conductivity. Their unique geometrical shape and morphology cause CNWs to possibly be an interesting material for field emitters [14]. Field emitters based on CNWs are expected to be free from Joule heating, in contrast to structures based on carbon nanotubes [15]. Good cooperation with gold nanoparticles has resulted in the development of a new type of Surface Enhanced Raman Scattering (SERS) substrate based on CNWs which is known for its high sensitivity [16]. The additional use of H-termination makes CNWs hydrophobic and very stable in a humid environment [17]. Zhang et al. [18] have shown that vertically aligned graphene can deliver superior thermal management capabilities, which has been revealed by scalable frost removal. Moreover, that effect was achieved on glass substrates, creating potentials for future transparent ’green-warmth’ devices.
Nevertheless, standard chemical vapor deposition (CVD) fabrication of CNWs usually requires a relatively high temperature of up to 1000 °C of growth or catalyst on the substrates (e.g., Cu or Ni) to obtain effective films [11]. This usually results in optically opaque films which are useless in the field of optical application. The solution is the utilization of plasma-enhanced processes at low temperatures, along with growth time limitation to minimize the absorbance of CNW layers [11,19,20,21]. The uniform and direct growth of few-layer graphene on a CuNi grid on the float glass has been demonstrated at the grown temperature of 500 °C by Chen et al. [21]. Furthermore, carbon nanowalls are wall-like “graphitic” sheets [22] that can also be fabricated by catalyst-free direct growth methods using fused silica as a substrate by radio frequency (plasma enhanced chemical vapor deposition (PECVD)). Nong et al. [22] have revealed that CNWs post-decorated with CdTe can work as a high-performance photo-anode with a current density of 3 mA cm−2.
Recently, authors have reported a novel way to achieve PECVD growth of enhanced carbon nanowalls on silicon wafers by in-situ boron doping, which has attracted interest due to a tunable band gap, high conductivity, high mechanical robustness and, unluckily, high optical absorbance [5,6,23]. For this reason, together with boron-doped nanocrystalline diamond thin films, their growth over a transparent substrate, such as quartz, is of current interest.
Growing doped-diamond or carbon nanowall films at low temperatures (less than 500 °C) is a main concern because many substrate materials, such as borosilicate glass, are unstable at higher temperatures, which are generally required for standard CVD diamond growth. However, the temperature affects the morphology of the nanomaterial. For this reason, Remes et al. investigated how the addition of oxygen to the gas mixture in a CVD setup allows for the growing of nanodiamond film at relatively low temperatures, which are, however, not conductive because the oxygen in plasma prevents the incorporation of boron into the diamond lattice [24].
A change in the conductivity of almost ten orders of magnitude was found by Gajewski et al. for a change in the boron concentration by five orders of magnitude, and in this study the different conduction mechanisms predominating at different boron doping levels were discussed [25].
In this paper, we demonstrate the direct growth of boron-doped nanowalls on optical grade fused quartz. Optical grade fused quartz is commonly used as a transparent and insulating amorphous oxide, with high surface hydrophilicity and low thermal conductivity in various optical and electronics devices. Merging glass with CNWs enables the fabrication of rigid transparent conductive electrodes for a number of applications. The growth of boron-doped carbon nanowalls (B-CNWs) with different doping concentrations (0, 1.2, 2, 5, and 7.5 part per thousand of [B]/[C] ratio) and different heating temperatures (400 °C, 550 °C, 700 °C, and 850 °C) was investigated in particular. The influence of temperature growth and boron on the structure of the obtained material, surface morphology, molecular composition, and electrical and optical properties are the focus of this paper. To the best of our knowledge, the effects of B-CNW growth on optical grade fused quartz for optical applications have not yet been reported.

2. Materials and Methods

2.1. B-CNWs Growth Method

Prior to CVD growth, fused quartz substrates (Continental Trade Sp.z.o.o., Warszawa, Poland) were pre-treated using the microwave PECVD (MWPECVD) system (SEKI Technotron AX5400S, Tokyo, Japan) for 20 min with H2 at 500 °C and 1000 W microwave power. This hydrogenation pre-treatment was supposed to change surface termination and wetting properties, which improve diamond seeding efficiency. Before the process, the substrates were seeded by spin-coating them in a diamond slurry [6]. The base pressure inside the chamber was 10−4 Torr. Several B-CNW films were fabricated using the following process conditions: gas mixtures H2, CH4, B2H6, and N2 with a total flow of 328 sccm; process pressure of 50 Torr; microwave power up to 1300 W; and microwave radiation of 2.45 GHz. For boron-doped samples, diborane (B2H6) was used at different levels (0, 1.2, 2, 5, and 7.5 part per thousand of [B]/[C] ratio) as an acceptor precursor. During the process, the substrate holder was heated up to the desired temperature by an induction heater (400 °C, 550 °C, 700 °C, and 850 °C) which was controlled by a thermocouple. Initially, three samples were grown for 7.5, 15, and 30 min (at 700 °C and 2000 ppm [B]/[C]) in order to choose the best process duration in terms of light transmittance and electrical conductivity. A 15 min process was chosen in order to meet both needs.
All the sample characteristics are summarized in Table 1.

2.2. Surface Morphology

Scanning electron microscopy via a FEI Quanta FEG 250 scanning electron microscope (SEM, FEI, Hillsboro, OR, USA), using a 15 kV beam accelerating voltage with a secondary electron–Everhart-Thornley (SE-ETD) detector working in high vacuum mode (pressure 10−4 Pa) was used to observe the structure of the B-CNW surfaces. The program used for data visualization and analysis was Gwyddion (v.2.40, Czech Metrology Institute, Brno, Czech Republic).

2.3. Raman Spectroscopy

The molecular composition of the deposited films was studied by means of Raman spectroscopy using a Raman microscope (InVia, Renishaw, UK). Spectra were recorded over the range 200–3500 cm−1 with an integration time of 5 s (10 averages) using an argon ion laser emitting at 514 nm and operating at 5% of its total power (50 mW). Data were smoothed (using a Savitzky-Golay method: 15 points, second polynomial order) and the baseline (approximated with a cubic polynomial) subtracted and normalized.

2.4. Spectroscopy Ellipsometry

Spectroscopic ellipsometry analysis was conducted with a Jobin-Yvon UVISEL phase-modulated ellipsometer (HORIBA Jobin-Yvon Inc., Edison, Rosemead, CA, USA). The investigated wavelength region was between 250 and 800 nm. The experiments were carried out at room temperature using an angle of incidence fixed at 60° and a compensator set at 45°. DeltaPsi software (v. 2.4.3, HORIBA Jobin-Yvon Inc., Edison, Rosemead, CA, USA) was employed to determine the spectral distributions of refractive index n (λ) and extinction coefficient k (λ) of the B-CNW films.

2.5. Electrical Conductivity

Electrical conductivities were measured at room temperature by a four-point probe placed in a straight line with equal spacing (s = 1.5 mm). Needle-like probes with a radius of 100 μm were utilized. The size of the samples was 1 × 1 cm2. A correction factor of 0.86 was considered during conductivity estimation, due to the finite sample size, and the layer thickness was estimated by spectroscopic ellipsometry measurements. The current was gradually increased from 0 up to 300 μA, with a step of 10 μA, with a source meter, and the voltage on the internal probes was measured with a Keithley 2400.

2.6. UV Visible Spectroscopy

UV-visible spectroscopy was measured using a double beam spectrophotometer (UV-9000 Metash, Shanghai, China) for the 200–1000 nm range with a scan step of 1 nm and a scan filter of 10. In this spectrophotometer, a deuterium lamp and a tungsten halogen lamp are used as light sources, a double beam optical system with 1200 lines/mm grating is implemented, and silicon photodiodes play the role of detectors. The wavelength repeatability is about 0.2 nm and the wavelength accuracy is equal to ±0.3 nm. Photometric accuracy is equal to about ±0.3 %T, and photometric repeatability is equal to 0.2 %T, where %T is percent transmittance.
In order to evaluate the band gap energy (Eg) of the samples, (αhν)n were plotted against the photon energy (hν), according to the well-known relation [26]
( α h ν ) n = A ( h ν E g ) ,
where A is a constant, hν is the photon energy, and n depends on the type of allowed transition in the material. It has a value equal to 1/2, 2, and 3/2 for directly allowed transitions, indirectly allowed transitions, and directly forbidden transitions, respectively.
While both allowed direct and indirect transitions were computed, those of a direct type are proposed in this study.

3. Results

The achieved transparency of B-CNW growth on quartz is shown in Figure 1, which shows a picture of the sample growth at 700 °C with a 2000 ppm [B]/[C] ratio.

3.1. Investigation of the Growth Process

Morphology of boron-doped carbon nanowalls plays an important role in the light transmission process and also affects the conductivity of the deposited material. Figure 2a–d shows the SEM images of B-CNW growth, respectively, at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio and for Figure 2c,e–h at 0, 1200, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C. The size of the B-CNWs is 1 cm × 1 cm.
It was found that a randomly vertically aligned wall structure belonged to the substrate only for samples with a temperature of process higher than 700 °C. B-CNWs are homogeneously distributed all over the substrate and they have sharp top edges.
For B-CNWs with a temperature of process of 400 or 550 °C the structure resembles nanoislands—one of the growth stages suggested by Hiramatsu et al. [27].
In our studies, a significant effect of temperature on B-CNW length was observed (Figure 3a). Samples with a temperature of process of 850 °C contain nanowalls approximately two times longer than for 700 °C samples. The distance between longer B-CNWs is greater than between the shorter ones. Temperature causes a decrease in the thickness of B-CNWs, which is correlated with the length of the nanowalls.
Boron incorporation, in different ratios at the same growth temperature, into the B-CNWs lattice causes a slight decrease in the thickness of B-CNWs (Figure 3b), which is in good agreement with research suggested by Sobaszek et al. [6].
It is worth pointing out that wall length is slightly positively influenced by the boron level in the gas phase. The sample 5000 ppm [B]/[C] at 700 °C has approximately 20 nm longer walls than the sample 0 ppm [B]/[C] at the same temperature of process.

3.2. Absorbance Spectrum

Absorbance spectra for sample growth at different temperatures are shown in Figure 4a.
The absorbance for wavelengths of between 400 nm and 700 nm ranges between 0.2 and 0.8 with increasing growth temperature. In particular, a prominent change in average absorbance is observed in the 200 nm to 400 nm wavelength region (Figure 4b). This is due to a change in the morphology and composition of the B-CNW layer, as confirmed by SEM (Figure 2) and Raman (Figure 5). As the temperature rises, we see a more distinct shape of the walls. Also as the temperature rises, we get an absorption peak at the wavelength of 200–350 nm. The absorption for 850 °C for 270 nm is 2.4, which corresponds to a transmission below 0.002%. This spectroscopic feature consistently observed in the UV range is known to originate from the peak in the joint density of states for a simple graphene layer [28] which occurs at the M point of the Brillouin zone at E = 2γ0 and is usually known as the plasmon resonance. For carbon nanotubes, this feature becomes shifted and split due to the more complex band structure, as has been predicted by several authors [29,30].
The absorbance spectrum for the samples with different [B]/[C] ratios are similar (Figure 4c), while the trend of visible light absorption for samples initially increases and then decreases with a higher [B]/[C] ratio higher than 5000 ppm (Figure 4d).

3.3. Raman Spectroscopy

Raman spectra of B-CNWs were analyzed and are reported in Figure 5. In all samples, two main bands at ∼1580 cm−1 and ∼1350 cm−1 are found, which are generally attributed to the G and D bands, respectively. In particular, Ferrari and Robertson have suggested that the G and D peaks are due to sp2 only [31].
The band centered near 1350 cm−1 corresponds to the breathing mode of sp2 atoms in a ring (D band), and Figure 5a and its intensity correlates with the amount of disorder of sp2-hybridized atoms in graphite-like materials. The different samples morphology, previously described and reported in Figure 2, is also highlighted by the presence of the D peak at 1350 cm−1 in the Raman spectra for the B-CNW growth at a higher temperature, which corresponds to distortion of the sp2 crystal structure; by contrast, for the first two samples (at 400 °C and 550 °C), a peak appears earlier, at 1334 cm−1, which can be attributed, instead, to the diamond structure [32].
The wide band in the range 1500–1600 cm−1 is dominated by overlapping G and D’ bands.
The G band centered at 1580 cm−1 is associated with bond stretching of sp2 atoms in rings and chains (G band, Figure 5b). The G peak position is shifted to a higher frequency with higher temperatures and the full-width at half-maximum (G-FWHW) is also found to decrease with temperature. Marchon et al. have reported a similar trend and have linked it to a decrease in sp3 content [33].
The D’ band observed near 1500 cm−1 is usually caused by defects generated via double-resonance processes. The origin of the D’ band in the plasma processed graphite nanomaterials can be associated with nitrogen defects incorporated into the graphene lattice [34,35]. The intensity of the D’ band changes with plasma process temperature. The maximal intensity is observed for B-CNW film synthesized at 400 °C and the band disappears for films deposited at temperatures above 700 °C. Increasing the process temperature results in a reduction of defect concentration, which is also reflected in the narrowing of the D band.
The band at 1220 cm−1 is reported to be caused by the effect of boron on the diamond lattice [36]. However, this peak also appears in boron-free CNWs, which makes another hypothesis reasonable. Chen et al. [37] merged their results with theoretical analysis and experimental results from others to identify two additional Raman peaks at around 1168 cm−1 and 1271 cm−1, in tetrahedral amorphous carbon, linked to the sp3 bonding. In our results, reported in Figure 5c, it is possible to observe a distinct peak, ahead of the D band, which redshifts with increasing temperature. This peak can be assigned to the sp3 carbons or disordered diamonds and is related to the phonon density of states (PDOS) band [38,39]. Moreover, from the Raman spectra it may be observed that when the boron concentration was increased further from a 2000 ppm [B]/[C] the G band peak upshifted by 6 cm−1. A similar result was noted by McGuire et al. [40] for boron-doped single-walled carbon nanotubes.

3.4. Optical and Electrical Properties

In Figure 6a it is possible to observe how higher electrical conductivity belongs to sample growth at a higher temperature, in a similar fashion to nanowall length, as this parameter particularly affects charge mobility. Longer wall structure delivers higher conductivity, mostly due to the minimized effect of carrier scattering at the inter-wall regions and surface defects. Next, the optical bandgap shows a maximum for the sample growth at 700 °C, which is much larger than the values reported by Kawai et al. [41]. This effect is unrevealed, though it could be attributed to the specific molecular structure caused by boron doping. Boron incorporation into the carbon lattice slightly positively affects nanowall length, which is not directly translated into an enhancement of the electrical conductivity; however, the latter, jointly with the optical bandgap, depends on the [B]/[C] ratio (Figure 6b). Overall, the incorporation of boron into the CNW lattice structure induces the unique effect of enhanced electrochemical performance and improved charge transfer [42,43].
The refractive index of B-CNWs, evaluated at 550 nm, ranges between 2.10 and 2.86 for sample growth at 700 °C, respectively, at 0 ppm and 5000 ppm boron doping levels; these results are comparable to those found by others [44,45]. Temperature also affects the refractive index; however, the variation is smaller and it falls within the previously reported range. The extinction coefficient shows a similar trend, reaching its minimum, equal to 0.83, with the sample growth at 700 °C and 0 ppm and 7500 ppm boron doping levels, and its maximum, equal to 1.24, with the 2000 ppm sample. For sample growth at a temperature of 300 °C and 450 °C, which does not exhibit a nanowall structure, the extinction coefficient is much lower, indicating that the structure is similar to that of diamond-like carbon (DLC) film [46].

4. Discussion

Process duration affects mainly the thickness of the nanowall layer. Longer times lead to thicker layers, together with longer and more electrically conductive nanowalls, while light transmittance is negatively affected. For these reasons, the right thickness is the starting point for obtaining a conductive and transparent composite.
Increasing nanowall length and layer thickness in accordance with boron doping are in contradiction to that reported by Takashi et al. [47] but in agreement with others [31,35,48].
Raman spectra and SEM pictures show that growing B-CNWs in low temperatures brings more defects than with elevated temperatures, with difficulties in developing a well-developed nanowall network on the substrate for temperatures lower than 700 °C, as well as a thinner B-CNW layer. Nanowall length and electrical conductivity are favorable with elevated growth temperatures.
The drop in growth rate versus stage temperature is caused by different surface pyrolysis reaction pathways involving H, CHx, HCN, and CN radicals [6]. The higher temperature favors bonding of CHx radicals towards the formation of a nanocrystalline diamond sp3 phase observed in the Raman spectra. The growth rate of the diamond phase is much smaller than the nanowall formation kinetics [6].
The dependency of B-CNW average absorbance in the 400–700 nm range, as a function of the conductance, is reported in Figure 7. It is interesting to observe how the conductance and absorbance are slightly negatively correlated for different boron concentrations (blue ●), while they are positively correlated for different growth temperatures (orange △).

5. Conclusions

In this study, a successful deposition of B-CNWs on a quartz glass substrate was conducted and characterization was carried out in order to study two parameters which strongly affect B-CNW growth and morphology: growth temperature and boron doping.
Process duration affects not only the thickness of the nanowall layer but also the development of the nanowall structure.
Raman spectrum and SEM pictures show that growing B-CNW in low temperatures brings more defects than with elevated temperatures, with difficulties in developing a well-developed nanowall network on the substrate observed for temperatures lower than 700 °C. Nanowall length and electrical conductivity are favorable with elevated growth temperatures.
Boron incorporation into the carbon lattice slightly positively affects nanowall length, which is not explicitly translated into an enhancement of the electrical conductivity.
These results suggest that it is possible to operate with both parameters to obtain a transparent and conductive film; however, boron doping is a preferred solution to maintain the transparency in the visible region, while a higher growth temperature is more effective to improve conductance.

Author Contributions

Conceptualization, M.P. and R.B.; sample growth, M.P. and M.F.; SEM analysis, M.R. and J.K.; Raman studies, M.S.; writing—original draft preparation, M.P. and M.R.; writing—review and editing, M.P., R.B., and M.F.; visualization, M.P. and M.S.; supervision, R.B. and M.L.R.; project administration, R.B.; funding acquisition, R.B. and M.L.R.

Funding

The authors gratefully acknowledge the financial support received from the Polish National Science Centre (NCN) under grant nos. 2016/21/B/ST7/01430, 2016/22/E/ST7/00102, and 2014/14/M/ST5/00715.

Acknowledgments

This work was partially supported by the Science for Peace Program of NATO (grant no. G5147). The DS funds of the Faculty of Electronics, Telecommunications, and Informatics of the Gdansk University of Technology are also acknowledged.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Lu, H.; Ren, X.; Ouyang, D.; Choy, W.C.H. Emerging Novel Metal Electrodes for Photovoltaic Applications. Small 2018, 14, 1703140. [Google Scholar] [CrossRef] [PubMed]
  2. Huang, Q.; Zhu, Y. Printing Conductive Nanomaterials for Flexible and Stretchable Electronics: A Review of Materials, Processes, and Applications. Adv. Mater. Technol. 2019, 1800546. [Google Scholar] [CrossRef]
  3. Jo, G.; Choe, M.; Cho, C.-Y.; Kim, J.H.; Park, W.; Lee, S.; Hong, W.-K.; Kim, T.-W.; Park, S.-J.; Hong, B.H.; et al. Large-scale patterned multi-layer graphene films as transparent conducting electrodes for GaN light-emitting diodes. Nanotechnology 2010, 21, 175201. [Google Scholar] [CrossRef] [PubMed]
  4. Wang, Z.; Mao, S.; Baba, K.; Ito, T.; Ogata, H. Microwave plasma-assisted regeneration of carbon nanosheets with bi- and trilayer of graphene and their application to photovoltaic cells. Carbon 2014, 67, 326–335. [Google Scholar] [CrossRef]
  5. Hosu, I.S.; Sobaszek, M.; Ficek, M.; Bogdanowicz, R.; Drobecq, H.; Boussekey, L.; Barras, A.; Melnyk, O.; Boukherroub, R.; Coffinier, Y. Carbon nanowalls: A new versatile graphene based interface for the laser desorption/ionization-mass spectrometry detection of small compounds in real samples. Nanoscale 2017, 9, 9701–9715. [Google Scholar] [CrossRef] [PubMed]
  6. Sobaszek, M.; Siuzdak, K.; Ryl, J.; Sawczak, M.; Gupta, S.; Carrizosa, S.B.; Ficek, M.; Dec, B.; Darowicki, K.; Bogdanowicz, R. Diamond Phase (sp3-C) Rich Boron-Doped Carbon Nanowalls (sp2-C): Physicochemical and Electrochemical Properties. J. Phys. Chem. C 2017, 121, 20821–20833. [Google Scholar] [CrossRef]
  7. Hassan, S.; Suzuki, M.; Mori, S.; El-Moneim, A.A. MnO2/carbon nanowalls composite electrode for supercapacitor application. J. Power Sources 2014, 249, 21–27. [Google Scholar] [CrossRef]
  8. Lin, G.; Zhou, Y.; Wang, Y.; Yan, X.; Wu, B.; Huang, F.; Fu, J.; Cheng, Q.; Yun, D. Direct growth of graphene nanowalls on quartz substrates as transparent conductive electrodes for perovskite solar cells. Funct. Mater. Lett. 2017, 11, 1850009. [Google Scholar] [CrossRef]
  9. Lee, K.-T.; Park, D.; Baac, H.; Han, S.; Lee, K.-T.; Park, D.H.; Baac, H.W.; Han, S. Graphene- and Carbon-Nanotube-Based Transparent Electrodes for Semitransparent Solar Cells. Materials 2018, 11, 1503. [Google Scholar] [CrossRef]
  10. Manawi, Y.M.; Ihsanullah; Samara, A.; Al-Ansari, T.; Atieh, M.A. A Review of Carbon Nanomaterials’ Synthesis via the Chemical Vapor Deposition (CVD) Method. Materials 2018, 11, 822. [Google Scholar] [CrossRef]
  11. Davami, K.; Shaygan, M.; Kheirabi, N.; Zhao, J.; Kovalenko, D.A.; Rümmeli, M.H.; Opitz, J.; Cuniberti, G.; Lee, J.-S.; Meyyappan, M. Synthesis and characterization of carbon nanowalls on different substrates by radio frequency plasma enhanced chemical vapor deposition. Carbon 2014, 72, 372–380. [Google Scholar] [CrossRef]
  12. Santhosh, N.; Filipič, G.; Tatarova, E.; Baranov, O.; Kondo, H.; Sekine, M.; Hori, M.; Ostrikov, K.; Cvelbar, U.; Santhosh, N.M.; et al. Oriented Carbon Nanostructures by Plasma Processing: Recent Advances and Future Challenges. Micromachines 2018, 9, 565. [Google Scholar] [CrossRef] [PubMed]
  13. Al-Jumaili, A.; Alancherry, S.; Bazaka, K.; Jacob, M.; Al-Jumaili, A.; Alancherry, S.; Bazaka, K.; Jacob, M.V. Review on the Antimicrobial Properties of Carbon Nanostructures. Materials 2017, 10, 1066. [Google Scholar] [CrossRef] [PubMed]
  14. Wu, Y.; Yang, B.; Zong, B.; Sun, H.; Shen, Z.; Feng, Y. Carbon nanowalls and related materials. J. Mater. Chem. 2004, 14, 469. [Google Scholar] [CrossRef]
  15. Teii, K.; Nakashima, M. Synthesis and field emission properties of nanocrystalline diamond/carbon nanowall composite films. Appl. Phys. Lett. 2010, 96, 023112. [Google Scholar] [CrossRef]
  16. Dyakonov, P.; Mironovich, K.; Svyakhovskiy, S.; Voloshina, O.; Dagesyan, S.; Panchishin, A.; Suetin, N.; Bagratashvili, V.; Timashev, P.; Shirshin, E.; et al. Carbon nanowalls as a platform for biological SERS studies. Sci. Rep. 2017, 7, 13352. [Google Scholar] [CrossRef] [PubMed]
  17. Krivchenko, V.A.; Evlashin, S.A.; Mironovich, K.V.; Verbitskiy, N.I.; Nefedov, A.; Wöll, C.; Kozmenkova, A.Y.; Suetin, N.V.; Svyakhovskiy, S.E.; Vyalikh, D.V.; et al. Carbon nanowalls: The next step for physical manifestation of the black body coating. Sci. Rep. 2013, 3, 3328. [Google Scholar] [CrossRef]
  18. Zhang, N.; Li, J.; Liu, Z.; Yang, S.; Xu, A.; Chen, D.; Guo, Q.; Wang, G. Direct synthesis of vertical graphene nanowalls on glass substrate for thermal management. Mater. Res. Express 2018, 5, 065606. [Google Scholar] [CrossRef] [Green Version]
  19. Pierpaoli, M.; Lewkowicz, A.; Ficek, M.; Ruello, M.L.; Bogdanowicz, R. Preparation and characterization of TiO2/carbon nanowall composite on a transparent substrate. Photonics Lett. Pol. 2018, 10, 54–56. [Google Scholar] [CrossRef]
  20. Zhao, R.; Ahktar, M.; Alruqi, A.; Dharmasena, R.; Jasinski, J.B.; Thantirige, R.M.; Sumanasekera, G.U. Electrical transport properties of graphene nanowalls grown at low temperature using plasma enhanced chemical vapor deposition. Mater. Res. Express 2017, 4, 055007. [Google Scholar] [CrossRef]
  21. Chen, Y.-Z.; Medina, H.; Tsai, H.-W.; Wang, Y.-C.; Yen, Y.-T.; Manikandan, A.; Chueh, Y.-L. Low Temperature Growth of Graphene on Glass by Carbon-Enclosed Chemical Vapor Deposition Process and Its Application as Transparent Electrode. Chem. Mater. 2015, 27, 1646–1655. [Google Scholar] [CrossRef]
  22. Nong, J.; Wei, W.; Song, X.; Tang, L.; Yang, J.; Sun, T.; Yu, L.; Luo, W.; Li, C.; Wei, D. Direct growth of graphene nanowalls on silica for high-performance photo-electrochemical anode. Surf. Coat. Technol. 2017, 320, 579–583. [Google Scholar] [CrossRef]
  23. Sankaran, K.J.; Ficek, M.; Kunuku, S.; Panda, K.; Yeh, C.-J.; Park, J.Y.; Sawczak, M.; Michałowski, P.P.; Leou, K.-C.; Bogdanowicz, R.; et al. Self-organized multi-layered graphene–boron-doped diamond hybrid nanowalls for high-performance electron emission devices. Nanoscale 2018, 10, 1345–1355. [Google Scholar] [CrossRef] [PubMed]
  24. Remes, Z.; Avigal, Y.; Kalish, R.; Uzan-Saguy, C.; Chack, A.; Nesládek, M. Structural, optical and electrical properties of nanodiamond films deposited by HFCVD on borosilicate glass, fused silica and silicon at low temperature. Phys. Status Solidi 2004, 201, 2499–2502. [Google Scholar] [CrossRef]
  25. Gajewski, W.; Achatz, P.; Williams, O.A.; Haenen, K.; Bustarret, E.; Stutzmann, M.; Garrido, J.A. Electronic and optical properties of boron-doped nanocrystalline diamond films. Phys. Rev. B 2009, 79, 045206. [Google Scholar] [CrossRef]
  26. Tauc, J. Optical properties and electronic structure of amorphous Ge and Si. Mater. Res. Bull. 1968, 3, 37–46. [Google Scholar] [CrossRef]
  27. Hiramatsu, M.; Hori, M. Fabrication of Carbon Nanowalls Using Novel Plasma Processing. Jpn. J. Appl. Phys. 2006, 45, 5522–5527. [Google Scholar] [CrossRef]
  28. Pedersen, T.G. Variational approach to excitons in carbon nanotubes. Phys. Rev. B 2003, 67, 073401. [Google Scholar] [CrossRef]
  29. Dmitrović, S.; Vuković, T.; Nikolić, B.; Damnjanović, M.; Milošević, I. Plasmon excitations of single-wall carbon nanotubes. Phys. Rev. B 2008, 77, 245415. [Google Scholar] [CrossRef]
  30. Takagi, Y.; Okada, S. Theoretical calculation for the ultraviolet optical properties of single-walled carbon nanotubes. Phys. Rev. B 2009, 79, 233406. [Google Scholar] [CrossRef] [Green Version]
  31. Ferrari, A.C.; Robertson, J.; Ferrari, O.; Robertson, J.O.H.N. Raman spectroscopy of amorphous, nanostructured, diamond-like carbon, and nanodiamond. Philos. Trans. A Math. Phys. Eng. Sci. 2004, 15, 2477–2512. [Google Scholar] [CrossRef] [PubMed]
  32. Haubner, R.; Moritz, R. Raman characterisation of diamond coatings using different laser wavelengths. In Proceedings of the Nineteenth European Conference on Chemical Vapor Deposition, Varna, Bulgaria, 1–6 September 2013; Volume 46, pp. 71–78. [Google Scholar]
  33. Marchon, B.; Gui, J.; Grannen, K.; Rauch, G.C. Photoluminescence and ramana Spectroscopy in hydrogenated carbon films. IEEE Trans. Magn. 1997, 33, 3149–3150. [Google Scholar] [CrossRef]
  34. Ye, D.; Wu, S.-Q.; Yu, Y.; Liu, L.; Lu, X.-P.; Wu, Y. Patterned graphene functionalization via mask-free scanning of micro-plasma jet under ambient condition. Appl. Phys. Lett. 2014, 104, 103105. [Google Scholar] [CrossRef]
  35. Bokobza, L.; Bruneel, J.-L.; Couzi, M.; Thakur, V.K. Raman Spectra of Carbon-Based Materials (from Graphite to Carbon Black) and of Some Silicone Composites. C 2015, 1, 77–94. [Google Scholar] [CrossRef]
  36. Krivchenko, V.A.; Lopaev, D.V.; Minakov, P.V.; Pirogov, V.G.; Rakhimov, A.T.; Suetin, N.V. Study of polycrystalline boron-doped diamond films by Raman spectroscopy and optical absorption spectroscopy. Tech. Phys. 2007, 52, 1471–1474. [Google Scholar] [CrossRef]
  37. Chen, Z.Y.; Zhao, J.P.; Yano, T.; Ooie, T.; Yoneda, M.; Sakakibara, J. Observation of sp3 bonding in tetrahedral amorphous carbon using visible Raman spectroscopy. J. Appl. Phys. 2000, 88, 2305–2308. [Google Scholar] [CrossRef]
  38. Windl, W.; Pavone, P.; Karch, K.; Schütt, O.; Strauch, D.; Giannozzi, P.; Baroni, S. Second-order Raman spectra of diamond from ab initio phonon calculations. Phys. Rev. B 1993, 48, 3164–3170. [Google Scholar] [CrossRef]
  39. Roy, D.; Barber, Z.H.; Clyne, T.W. Ag nanoparticle induced surface enhanced Raman spectroscopy of chemical vapor deposition diamond thin films prepared by hot filament chemical vapor deposition. J. Appl. Phys. 2002, 91, 6085–6088. [Google Scholar] [CrossRef]
  40. McGuire, K.; Gothard, N.; Gai, P.; Dresselhaus, M.; Sumanasekera, G.; Rao, A. Synthesis and Raman characterization of boron-doped single-walled carbon nanotubes. Carbon 2005, 43, 219–227. [Google Scholar] [CrossRef]
  41. Kawai, S.; Kondo, S.; Takeuchi, W.; Kondo, H.; Hiramatsu, M.; Hori, M. Optical properties of evolutionary grown layers of carbon nanowalls analyzed by spectroscopic ellipsometry. Jpn. J. Appl. Phys. 2010, 49, 0602201–0602203. [Google Scholar] [CrossRef]
  42. Siuzdak, K.; Ficek, M.; Sobaszek, M.; Ryl, J.; Gnyba, M.; Niedziałkowski, P.; Malinowska, N.; Karczewski, J.; Bogdanowicz, R. Boron-Enhanced Growth of Micron-Scale Carbon-Based Nanowalls: A Route toward High Rates of Electrochemical Biosensing. ACS Appl. Mater. Interfaces 2017, 9, 12982–12992. [Google Scholar] [CrossRef] [PubMed]
  43. Fudala-Ksiazek, S.; Sobaszek, M.; Luczkiewicz, A.; Pieczynska, A.; Ofiarska, A.; Fiszka-Borzyszkowska, A.; Sawczak, M.; Ficek, M.; Bogdanowicz, R.; Siedlecka, E.M. Influence of the boron doping level on the electrochemical oxidation of raw landfill leachates: Advanced pre-treatment prior to the biological nitrogen removal. Chem. Eng. J. 2018, 334, 1074–1084. [Google Scholar] [CrossRef]
  44. Gharibyan, A.; Hayrapetyan, D.; Panosyan, Z.; Yengibaryan, Y. Preparation of wide range refractive index diamond-like carbon films by means of plasma-enhanced chemical vapor deposition. Appl. Opt. 2011, 50, G69. [Google Scholar] [CrossRef] [PubMed]
  45. Ficek, M.; Sobaszek, M.; Gnyba, M.; Ryl, J.; Gołuński, Ł.; Smietana, M.; Jasiński, J.; Caban, P.; Bogdanowicz, R. Optical and electrical properties of boron doped diamond thin conductive films deposited on fused silica glass substrates. Appl. Surf. Sci. 2016, 387, 846–856. [Google Scholar] [CrossRef]
  46. Robertson, J. Diamond-like amorphous carbon. Mater. Sci. Eng. Rep. 2002, 37, 129–281. [Google Scholar] [CrossRef] [Green Version]
  47. Itoh, T.; Nakanishi, Y.; Ito, T.; Vetushka, A.; Ledinský, M.; Fejfar, A.; Kočka, J.; Nonomura, S. Electrical properties of carbon nanowall films. J. Non-Cryst. Solids 2012, 358, 2548–2551. [Google Scholar] [CrossRef]
  48. Kurita, S.; Yoshimura, A.; Kawamoto, H.; Uchida, T.; Kojima, K.; Tachibana, M.; Molina-Morales, P.; Nakai, H. Raman spectra of carbon nanowalls grown by plasma-enhanced chemical vapor deposition. J. Appl. Phys. 2005, 97. [Google Scholar] [CrossRef]
Figure 1. Picture of the fabricated sample: growth at 700 °C with a 2000 ppm [B]/[C] ratio.
Figure 1. Picture of the fabricated sample: growth at 700 °C with a 2000 ppm [B]/[C] ratio.
Materials 12 00547 g001
Figure 2. Scanning electron microscopy (SEM) picture of B-CNW growth, respectively, at (a) 400 °C, (b) 550 °C, (c) 700 °C, and (d) 850 °C at 2000 ppm [B]/[C] ratio and with (e) 0, (f) 1200, (g) 5000, and (h) 7500 ppm [B]/[C] at 700 °C. Sample (c) belongs to both series.
Figure 2. Scanning electron microscopy (SEM) picture of B-CNW growth, respectively, at (a) 400 °C, (b) 550 °C, (c) 700 °C, and (d) 850 °C at 2000 ppm [B]/[C] ratio and with (e) 0, (f) 1200, (g) 5000, and (h) 7500 ppm [B]/[C] at 700 °C. Sample (c) belongs to both series.
Materials 12 00547 g002
Figure 3. (a) Nanowall length and layer thickness for B-CNW growth at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio; (b) nanowall length and layer thickness for B-CNW growth at 0, 1200, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C.
Figure 3. (a) Nanowall length and layer thickness for B-CNW growth at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio; (b) nanowall length and layer thickness for B-CNW growth at 0, 1200, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C.
Materials 12 00547 g003
Figure 4. (a) UV-visible absorbance spectrum and (b) 400–700 nm average absorbance for B-CNW growth at 400 °C, 550 °C, 700 °C, and 850 °C at 2000 ppm [B]/[C] ratio; (c) UV-visible absorbance spectrum and (d) 400–700 nm average absorbance for B-CNWs at 0, 1200, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C.
Figure 4. (a) UV-visible absorbance spectrum and (b) 400–700 nm average absorbance for B-CNW growth at 400 °C, 550 °C, 700 °C, and 850 °C at 2000 ppm [B]/[C] ratio; (c) UV-visible absorbance spectrum and (d) 400–700 nm average absorbance for B-CNWs at 0, 1200, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C.
Materials 12 00547 g004
Figure 5. Raman spectra of sample growth at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio. In the inserts (ac), peak position and full-width at half-maximum (FWHM) are reported.
Figure 5. Raman spectra of sample growth at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio. In the inserts (ac), peak position and full-width at half-maximum (FWHM) are reported.
Materials 12 00547 g005
Figure 6. (a) Optical bandgap and electrical conductivity for B-CNW growth at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio; (b) optical bandgap and electrical conductivity for B-CNW growth at 0, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C.
Figure 6. (a) Optical bandgap and electrical conductivity for B-CNW growth at 400 °C, 550 °C, 700 °C, and 850 °C at a 2000 ppm [B]/[C] ratio; (b) optical bandgap and electrical conductivity for B-CNW growth at 0, 2000, 5000, and 7500 ppm [B]/[C] at 700 °C.
Materials 12 00547 g006
Figure 7. Dependency of the average absorbance on the conductivity of B-CNWs deposited on fused quartz.
Figure 7. Dependency of the average absorbance on the conductivity of B-CNWs deposited on fused quartz.
Materials 12 00547 g007
Table 1. Parameters of growth of boron-doped carbon nanowall (B-CNW) films.
Table 1. Parameters of growth of boron-doped carbon nanowall (B-CNW) films.
Sample IDGrowth Time (min)Boron Doping
[B]/[C] (Part Per Thousand)
Furnace Temperature
(°C)
2k_700152700
0k_700150700
1.2k_700151.2700
5k_700155700
7.5k_700157.5700
152400
152550
152850

Share and Cite

MDPI and ACS Style

Pierpaoli, M.; Ficek, M.; Rycewicz, M.; Sawczak, M.; Karczewski, J.; Ruello, M.L.; Bogdanowicz, R. Tailoring Electro/Optical Properties of Transparent Boron-Doped Carbon Nanowalls Grown on Quartz. Materials 2019, 12, 547. https://doi.org/10.3390/ma12030547

AMA Style

Pierpaoli M, Ficek M, Rycewicz M, Sawczak M, Karczewski J, Ruello ML, Bogdanowicz R. Tailoring Electro/Optical Properties of Transparent Boron-Doped Carbon Nanowalls Grown on Quartz. Materials. 2019; 12(3):547. https://doi.org/10.3390/ma12030547

Chicago/Turabian Style

Pierpaoli, Mattia, Mateusz Ficek, Michał Rycewicz, Mirosław Sawczak, Jakub Karczewski, Maria Letizia Ruello, and Robert Bogdanowicz. 2019. "Tailoring Electro/Optical Properties of Transparent Boron-Doped Carbon Nanowalls Grown on Quartz" Materials 12, no. 3: 547. https://doi.org/10.3390/ma12030547

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop