Next Article in Journal
Preparation of Organo-Montmorillonite Modified Poly(lactic acid) and Properties of Its Blends with Wood Flour
Next Article in Special Issue
Polypyrrole Nanowires with Ordered Large Mesopores: Synthesis, Characterization and Applications in Supercapacitor and Lithium/Sulfur Batteries
Previous Article in Journal
Functionalization of Neutral Polypropylene by Using Low Pressure Plasma Treatment: Effects on Surface Characteristics and Adhesion Properties
Previous Article in Special Issue
Graphene-Based Thermal Interface Materials: An Application-Oriented Perspective on Architecture Design
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Enhanced Proton Conductivity in Sulfonated Poly(ether ether ketone) Membranes by Incorporating Sodium Dodecyl Benzene Sulfonate

Beijing Key Laboratory of Energy Safety and Clean Utilization, North China Electric Power University, Beijing 102206, China
*
Author to whom correspondence should be addressed.
Polymers 2019, 11(2), 203; https://doi.org/10.3390/polym11020203
Submission received: 3 January 2019 / Revised: 21 January 2019 / Accepted: 22 January 2019 / Published: 24 January 2019
(This article belongs to the Special Issue Conducting Polymers)

Abstract

:
It is of great importance to improve the proton conductivity of proton exchange membranes by easy-handling and cost-efficient approaches. In this work, we incorporated a commercially obtained surfactant, sodium dodecyl benzene sulfonate (SDBS), into sulfonated poly(ether ether ketone) (SPEEK) through solution casting to prepare SPEEK/SDBS membranes. When no more than 10 wt % SDBS was added, the SDBS was well dissolved into the SPEEK matrix, and the activation energy for the proton transfer in the SPEEK/SDBS membranes was greatly reduced, leading to significant enhancement of the membrane proton conductivity. Compared with the SPEEK control membrane, the SPEEK/SDBS membrane with 10 wt % SDBS showed a 78% increase in proton conductivity, up from 0.051 S cm−1 to 0.091 S cm−1, while the water uptake increased from 38% to 62%. Moreover, the SPEEK/SDBS membrane exhibited constant proton conductivity under a long-term water immersion test.

1. Introduction

Proton exchange membrane fuel cells (PEMFCs) have been considered a promising energy conversion device due to their advantages of high energy efficiency and low environmental impact [1]. Proton exchange membranes (PEMs) are the core components of PEMFCs, and proton conductivity is one of the most important properties for the PEMs [2,3]. Among the various PEMs, sulfonated poly(ether ether ketone) (SPEEK) has attracted great attention due to its good mechanical strength, high chemical stability, and low cost [4,5,6]. Generally, high proton conductivity can be achieved when SPEEK has a high degree of sulfonation (DS) [7,8], while the high DS also results in high water uptake, leading to poor dimensional stability.
A commonly used and effective way to improve the proton conductivity without much deterioration of the dimensional stability of SPEEK is to introduce inorganic fillers modified with sulfonate-containing components into the polymer matrix [9,10,11]. Such enhancements in proton conductivity are mostly due to the formation of additional proton transport pathways in the PEMs. For example, Liu et al. [12] utilized dopamine-initiated atom transfer radical polymerization to graft polystyrene sulfonic acid (PSSA) onto the surfaces of halloysite nanotubes (HNTs), and when adding 15 wt % of these modified HNTs, the proton conductivity of a SPEEK membrane at 25 °C increased by 54%. Jiang et al. [13] used sodium dodecyl benzene sulfonate (SDBS) adsorbed onto graphene oxide (GO) as a filler to enhance the proton conductivity of SPEEK, and the proton conductivity was increased from 39.5 mS cm−1 to 93.8 mS cm−1 by incorporating 8 wt % filler. However, the modification process of the inorganic filler is usually complicated and sometimes costly. Another effective method to improve the proton conductivity, especially under high temperature and low humidity, is to incorporate solid heteropolyacid (HPA) or liquid phosphoric acid (PA) into the PEMs [14,15]. Unfortunately, the easy leaching of HPA impedes the further application of HPA-filled composites as PEMs, so great efforts have been made to immobilize HPA [16,17,18,19,20], but these are still cost- and time-consuming.
Therefore, there is still a need to explore easy-handling and cost-efficient approaches to further improve the proton conductivity of SPEEK. SDBS is a kind of commonly used surfactant, with one end being hydrophilic and the other end being lyophilic, and the sulfonic acid groups of SDBS might facilitate the connecting of the hydrophilic phase of PEMs, resulting in enhanced proton conductivity. In this work, to create more proton transport pathways in SPEEK membranes, the commercially obtained surfactant SDBS was used to prepare SPEEK/SDBS membranes through solution casting. Molecular-level dispersion of a relatively high content of SDBS was obtained in the SPEEK matrix. The effects of the content of SDBS on the membrane behavior were extensively investigated in terms of ion exchange capacity (IEC), proton conductivity, water uptake, and mechanical properties.

2. Experimental

2.1. Materials

Poly(ether ether ketone) (PEEK) (Victrex 450PF) was purchased from Victrex (Lancashire, UK). SDBS (99%) and dimethylacetamide (DMAc) were provided by Alfa Aesar, Tianjian, China.

2.2. Sample Preparation

SPEEK was synthesized according to a method detailed in our previous work. To prepare SPEEK/SDBS membranes, both SPEEK and SDBS (with structural formulae shown in Figure 1a,b, respectively) were dissolved in DMAc, followed by stirring for 24 h at room temperature. After being degassed to remove air bubbles, the mixture was cast onto a flat glass substrate and dried at 80 °C for 24 h, and then further dried at 100 °C under vacuum for 18 h to thoroughly remove the DMAc. To replace the sodium ions of SDBS by H+, the as-prepared SPEEK/SDBS membranes with various SDBS contents were treated with 1 M H2SO4 and deionized (DI) water sequentially before use. For simplicity, the treated membranes were abbreviated as SPEEK/SDBS-x membranes, where x denotes the pre-introduced SDBS content (wt %).

2.3. Measurements

The sample cross section was obtained after breaking the membrane in liquid nitrogen followed by sputtering with gold. The morphology images were obtained via scanning electron microscopy (SEM) (SU8010, Hitachi Co. Ltd., Tokyo, Japan) at an accelerating voltage of 5 kV.
The IECs of the membranes were determined by an acid–base titration method according to the literature [21,22]. After immersing the dried membrane (~0.2 g) in 5.0 M NaCl solution (15 mL) for 24 h to release all H+, the amount of H+ was titrated with 0.01 M NaOH standard solution using phenolphthalein as an indicator. The IEC was calculated using the equation below:
I E C = V × c m ,
where V and c are the volume and concentration of NaOH solution, respectively, and m is the weight of the dried membrane. The DS of the SPEEK was calculated to be 54% (for comparison, a SPEEK membrane with a DS of 73% was also prepared) from the following equation described in the literature [23]:
D S = 288 × I E C 1000 102 × I E C × 100 % .
The dried membranes were immersed in deionized water at 25 °C for 6 h, and the wet membranes were obtained after the membranes were taken out and wiped with filter paper. The membrane water uptake was determined by the following equation:
W a t e r   u p t a k e = m w m d m d × 100 % ,
where md and mw are the masses of the dry and wet membranes, respectively.
Proton conductivity was calculated using the following equation:
σ = L R × w × δ ,
where L is the spacing between the two electrodes; w and δ are the width and thickness of the samples, respectively; and R is the resistance measured in water via an AC impedance technique using an electrochemical workstation (Zennium Pro., Zahner, Germany).
According to ISO 1184-1983, the stress–strain curves of the membranes were recorded using an electrical tensile tester (AI-7000S1, Goodtechwill Testing Machines, Co. Ltd., China) at the speed of 2 mm min−1 under the relative humidity of 20%.
All the measurements were conducted at 25 °C unless mentioned otherwise.

3. Results and Discussion

3.1. SEM Observation of SPEEK/SDBS Membranes

SEM images of SPEEK and SPEEK/SDBS membranes with various SDBS contents are shown in Figure 2. As can be seen from Figure 2a, the freeze-fracture surface of the SPEEK membrane is relatively smooth without any visible voids. It can also be observed from Figure 2b–d that the surface morphologies of the SPEEK/SDBS membranes with SDBS contents of 2 wt %, 4 wt %, and 10 wt % are quite similar to that of the SPEEK membrane. Such similarity indicates that the SDBS could be well dissolved in the SPEEK matrix when no more than 10 wt % SDBS is incorporated; this should be due to the amphiphilic nature of both SPEEK and SDBS and the formation of ion clusters between the sulfonic acid groups of SPEEK and SDBS. The formation of ion clusters between the components containing sulfonic acid groups has been commonly observed in the literature [24,25]. For comparison, the freeze-fracture surfaces of SPEEK/SDBS membranes with SDBS contents of 15 wt % and 20 wt %, as shown in Figure 2e,f, respectively, are relatively rough, and some voids with the size of ~1 μm can be seen. When a large amount of SDBS (SDBS content higher than 10 wt %) is introduced, exceeding the saturation degree of SDBS in the SPEEK matrix, some SDBS should dissolve out from the SPEEK matrix, resulting in the formation of SDBS aggregates. However, these undissolved SDBS aggregates could be washed away during the membrane pre-treatment with 1 M H2SO4 and DI water, as mentioned in the experimental section; therefore, there exist some voids in the SPEEK/SDBS membranes with high SDBS content.

3.2. IECs of SPEEK/SDBS Membranes

The IECs of the SPEEK/SDBS membranes with various SDBS contents are exhibited in Figure 3. The IECs of the SPEEK membrane and SDBS were determined to be 1.58 mmol g−1 and 3.06 mmol g−1, respectively. With increasing SDBS content, the IEC of the SPEEK/SDBS membranes first increases until it reaches a maximum of 1.82 mmol g−1 at 10 wt % SDBS content and then remains almost unchanged. Compared with SPEEK, SDBS exhibits a higher IEC, so the incorporation of SDBS into the SPEEK matrix could increase the IEC of the SPEEK/SDBS membranes. Additionally, we assume that the IECs of SPEEK/SDBS membranes linearly increase with increasing SDBS content; thus, the theoretical IECs of SPEEK/SDBS membranes should follow the dashed line shown in Figure 3, which is the connection between the IECs of SPEEK (SDBS content of 0 wt %) and SDBS (SDBS content of 100 wt %). However, it is found that the experimental IECs of SPEEK/SDBS membranes with no more than 10 wt % SDBS are much higher than the theoretical value, indicating that the protons for titrating are more dissociated than expected. Such a phenomenon should be attributed to the good dispersion of SDBS in the SPEEK matrix and the promotion of proton dissociation through ion clusters between SPEEK and SDBS when no more than 10 wt % SDBS is added. In comparison, when the SDBS content is higher than 10 wt % in the membranes, the leakage of undissolved SDBS occurs, as illustrated in the SEM observation mentioned above, which should not lead to an increase in the actual SDBS content in the membrane with further SDBS addition. As a result, the SPEEK/SDBS membranes with SDBS contents of 15 wt % and 20 wt % show almost the same IEC as the membrane with 10 wt % SDBS.

3.3. Proton Conductivity and Water Uptake of SPEEK/SDBS Membranes

The proton conductivity and water uptake of the SPEEK/SDBS membranes with various SDBS contents are exhibited in Figure 4. For the membrane water uptake, a gradual increase with SDBS is expected because the hygroscopic SDBS tends to absorb more water than does SPEEK, and the voids created by the leakage of SDBS are responsible for the slightly increased water uptake at high SDBS content. Moreover, with increasing SDBS content, the proton conductivity of the SPEEK/SDBS membranes greatly increases at first and then levels off, which is consistent with the change in the membrane IEC. Such an enhancement in the membrane proton conductivity with low SDBS addition should be due to two main factors. Firstly, SDBS has a higher IEC and thus can dissociate more protons than SPEEK, so the introduction of SDBS can create more continuous proton transfer channels in the membrane. Secondly, the formation of ion clusters between the sulfonic acid groups of SPEEK and SDBS could result in stronger dissociation of protons, further facilitating the hopping of protons. However, the actual SDBS content in the membrane does not increase with further increasing SDBS content above 10 wt %, thus leading to unchanged proton conductivity. It should be noted that the formation of ion clusters between the sulfonic acid groups of SPEEK and SDBS would not lead to an additional increase in water uptake. As a result, the SPEEK/SDBS membrane with 10 wt % SDBS exhibits much higher proton conductivity than the SPEEK membrane, with the proton conductivity rising from 0.051 S cm−1 to 0.091 S cm−1, while the water uptake increases from 38% to 62%. For comparison, the SPEEK membrane with a DS of 73% only achieves the proton conductivity of 0.082 S cm−1 with relatively high water uptake (80%). Although the enhancement in proton conductivity in our work was not as high as that of the previous reported SPEEK membrane using SDBS-adsorbed graphene oxide (GO) as a filler (the proton conductivity rising from 39.5 mS cm−1 to 93.8 mS cm−1 by using 8 wt % filler) [13], to improve the proton conductivity by directly incorporating SDBS into SPEEK is a more cost-efficient approach and is easier to handle.

3.4. Activation Energy for Proton Conduction in SPEEK/SDBS Membranes

The activation energy for proton conduction (Ea) reveals the minimum energy required for proton transport from one free site to another, and a low Ea indicates lower energy loss caused by ionic resistance of the membrane, which is beneficial for the energy utilization of PEMFCs [13]. Figure 5 shows the Arrhenius plots of proton conductivity (σ) for SPEEK and SPEEK/SDBS membranes with SDBS contents of 2 wt %, 4 wt %, and 10 wt %, and Ea (kJ mol−1) can be derived from the linear fitting of the plots using the following equation [26]:
ln σ = ln A E a R T ,
where A is the pre-exponential factor, R is the ideal gas constant (8.314 J K−1 mol−1), and T is the temperature (K).
As is well known, there are two main mechanisms [27,28,29,30]—Grotthuss and vehicle mechanisms—responsible for the proton transport in hydrated membranes. For the Grotthuss mechanism, protons jump between adjacent sulfonic acid groups or water molecules to achieve proton transfer, while for the vehicle mechanism, the protons are transferred by −SO3H and some complexes such as H3O+ and H5O2+. The calculated Ea for a SPEEK membrane is 19.7 kJ mol−1, which lies within the reported Ea range for the Grotthuss mechanism (14.0~40.0 kJ mol−1) [31], indicating that the proton conduction in the SPEEK membrane is mainly dominated by the Grotthuss mechanism. For comparison, the calculated Ea values for the SPEEK/SDBS-2, SPEEK/SDBS-4, and SPEEK/SDBS-10 membranes are 17.4 kJ mol−1, 12.3 kJ mol−1, and 10.7 kJ mol−1, respectively. These are lower than that of the SPEEK membrane and decrease with increasing SDBS content until the SDBS content reaches 10 wt %. When SDBS is added into the membrane, the hydrophilic sulfonic acid groups in SDBS contribute to the water absorption of the membranes, and more water molecules might help to construct a proton-conducting pathway and improve the proton transfer ability via the vehicle mechanism; therefore, much lower Ea values are achieved by the SPEEK/SDBS membranes. The proton transfer mechanisms, including the Grotthuss and vehicle mechanisms, in the SPEEK/SDBS membranes are shown in Figure 6.

3.5. Stability of SPEEK Nanocomposite Membranes

Generally, the leakage of water-soluble low-molecular-weight compounds in PEMs is extremely serious, so it is quite necessary to evaluate the stability of SDBS in the SPEEK membrane. The SPEEK/SDBS-2, SPEEK/SDBS-4, and SPEEK/SDBS-10 membranes were immersed in water that flowed continuously, and proton conductivities were tested at various times to check the stability of the membranes. As shown in Figure 7, the proton conductivities of the three SPEEK/SDBS membranes remained almost constant after 80 days, indicating that SDBS is quite stable in the membranes without leaking. Additionally, the weight of the membranes remains constant during the test, also illustrating that the SDBS could not have leaked out. These results can be explained as follows: SDBS is an amphiphilic molecule with one end being hydrophilic and the other end being lyophilic. The relatively long alkyl chain of SDBS can be entangled with hydrophobic-phase macromolecules in SPEEK, while the sulfonic acid groups of SDBS can form ionic clusters with the sulfonic acid groups in SPEEK. Therefore, the migration of SDBS would encounter large resistance in either the hydrophilic or the hydrophobic phase. The SEM images also confirm that SDBS is well embedded in SPEEK when the loading of SDBS does not exceed 10 wt %.

3.6. Mechanical Properties of SPEEK/SDBS Membranes

Tensile tests were performed to investigate the effect of SDBS on the mechanical properties of SPEEK/SDBS membranes, and the results are shown in Table 1. The stress–strain curves are presented in Figure 8. Compared to the SPEEK membrane, the SPEEK/SDBS membranes demonstrate lower elastic moduli, mainly due to the incorporation of soft organic SDBS acting as a plasticizer. The yield strength, tensile strength, and elongation at break of the SPEEK/SDBS membranes are also lower than those of the SPEEK membrane because the addition of SDBS may increase the space between the polymer chains, and the molecular inter-atomic force is thus damaged at some level. Nevertheless, the SPEEK/SDBS membranes still possess sufficiently high mechanical properties to be applied in fuel cells.

4. Conclusions

In this work, a commercially available surfactant, SDBS, was incorporated into SPEEK through solution casting to prepare SPEEK/SDBS membranes. As illustrated by SEM observations, SDBS was well dissolved into the SPEEK matrix when no more than 10 wt % SDBS was added, and leakage of SDBS occurred in the SPEEK/SDBS with SDBS content higher than 10%. By incorporating SDBS, the activation energy for the proton transfer in the membranes was greatly reduced due to the formation of more continuous proton transfer channels. Compared with the SPEEK control membrane, the SPEEK/SDBS membranes showed significantly enhanced proton conductivity with relatively low water uptake because the formation of ion clusters between the sulfonic acid groups of SPEEK and SDBS could promote proton dissociation without leading to an additional increase in water uptake. The proton conductivity of the SPEEK/SDBS membrane was constant during long-term water immersion tests.

Author Contributions

Conceptualization, J.L. and S.H.; methodology, W.D.; software, S.Z.; validation, S.H. and J.L.; formal analysis, S.Z. and L.C.; investigation, B.Z.; resources, J.L.; data curation, S.Z., W.D. and B.Z.; writing—original draft preparation, S.Z.; writing—review and editing, S.H. and J.L.; visualization, L.C.; supervision, S.H. and J.L.; project administration, S.H. and J.L.; funding acquisition, B.Z. and J.L.

Funding

This research was funded by the National Natural Science Foundation of China, 51773058 and 51776069, and the National Key Basic Research Program of China (973 Program), 2015CB932201. The APC was funded by the National Natural Science Foundation of China, 51773058.

Acknowledgements

This work was supported by the National Natural Science Foundation of China (51773058 and 51776069) and the National Key Basic Research Program of China (973 Program) (2015CB932201).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Mishra, A.K.; Bose, S.; Kuila, T.; Kim, N.H.; Lee, J.H. Silicate-based polymer-nanocomposite membranes for polymer electrolyte membrane fuel cells. Prog. Polym. Sci. 2012, 37, 842–869. [Google Scholar] [CrossRef]
  2. Cheng, T.; Zhang, X.; Ma, Y.; Huang, Y.; Liu, X. Constructing Continuous Proton-Conducting Highways within Sulfonated Poly(Arylene Ether Nitrile) Composite Membrane by Incorporating Amino-Sulfo-Bifunctionalized GO. Polymers 2018, 10, 1005. [Google Scholar] [CrossRef]
  3. Bose, S.; Kuila, T.; Nguyen, T.X.H.; Kim, N.H.; Lau, K.-T.; Lee, J.H. Polymer membranes for high temperature proton exchange membrane fuel cell: Recent advances and challenges. Prog. Polym. Sci. 2011, 36, 813–843. [Google Scholar] [CrossRef]
  4. Shukla, A.; Bhat, S.D.; Pillai, V.K. Simultaneous unzipping and sulfonation of multi-walled carbon nanotubes to sulfonated graphene nanoribbons for nanocomposite membranes in polymer electrolyte fuel cells. J. Membr. Sci. 2016, 520, 657–670. [Google Scholar] [CrossRef]
  5. Liu, X.; He, S.J.; Liu, S.X.; Jia, H.N.; Chen, L.; Zhang, B.; Zhang, L.Q.; Lin, J. The roles of solvent type and amount of residual solvent on determining the structure and performance of sulfonated poly(ether ether ketone) proton exchange membranes. J. Membr. Sci. 2017, 523, 163–172. [Google Scholar] [CrossRef]
  6. He, S.J.; Lin, Y.K.; Ma, H.F.; Jia, H.N.; Liu, X.; Lin, J. Preparation of sulfonated poly(ether ether ketone) (SPEEK) membrane using ethanol/water mixed solvent. Mater. Lett. 2016, 169, 69–72. [Google Scholar] [CrossRef]
  7. Lim, M.Y.; Kim, K. Sulfonated Poly(Arylene Ether Sulfone) and Perfluorosulfonic Acid Composite Membranes Containing Perfluoropolyether Grafted Graphene Oxide for Polymer Electrolyte Membrane Fuel Cell Applications. Polymers 2018, 10, 569. [Google Scholar] [CrossRef]
  8. Parnian, M.J.; Rowshanzamir, S.; Gashoul, F. Comprehensive investigation of physicochemical and electrochemical properties of sulfonated poly (ether ether ketone) membranes with different degrees of sulfonation for proton exchange membrane fuel cell applications. Energy 2017, 125, 614–628. [Google Scholar] [CrossRef]
  9. He, S.J.; Jia, H.N.; Lin, Y.K.; Qian, H.X.; Lin, J. Effect of clay modification on the structure and properties of sulfonated poly(ether ether ketone) (SPEEK)/clay nanocomposites. Polym. Compos. 2016, 37, 2632–2638. [Google Scholar] [CrossRef]
  10. Laberty-Robert, C.; Vallé, K.; Pereira, F.; Sanchez, C. Design and properties of functional hybrid organic-inorganic membranes for fuel cells. Chem. Soc. Rev. 2011, 40, 961–1005. [Google Scholar] [CrossRef] [PubMed]
  11. Tripathi, B.P.; Shahi, V.K. Organic-inorganic nanocomposite polymer electrolyte membranes for fuel cell applications. Prog. Polym. Sci. 2011, 36, 945–979. [Google Scholar] [CrossRef]
  12. Liu, X.; He, S.J.; Song, G.; Jia, H.N.; Shi, Z.Z.; Liu, S.X.; Zhang, L.Q.; Lin, J. Proton conductivity improvement of sulfonated poly(ether ether ketone) nanocomposite membranes with sulfonated halloysite nanotubes prepared via dopamine-initiated atom transfer radical polymerization. J. Membr. Sci. 2016, 504, 206–219. [Google Scholar] [CrossRef]
  13. Jiang, Z.; Zhao, X.; Fu, Y.; Manthiram, A. Composite membranes based on sulfonated poly(ether ether ketone) and SDBS-adsorbed graphene oxide for direct methanol fuel cells. J. Mater. Chem. 2012, 22, 24862–24869. [Google Scholar] [CrossRef]
  14. Choi, S.W.; Park, J.O.; Pak, C.; Choi, K.H.; Lee, J.C.; Chang, H. Design and Synthesis of Cross-Linked Copolymer Membranes Based on Poly(benzoxazine) and Polybenzimidazole and Their Application to an Electrolyte Membrane for a High-Temperature PEM Fuel Cell. Polymers 2013, 5, 77–111. [Google Scholar] [CrossRef] [Green Version]
  15. Park, C.H.; Lee, C.H.; Guiver, M.D.; Lee, Y.M. Sulfonated hydrocarbon membranes for medium-temperature and low-humidity proton exchange membrane fuel cells (PEMFCs). Prog. Polym. Sci. 2011, 36, 1443–1498. [Google Scholar] [CrossRef] [Green Version]
  16. He, S.J.; Liu, S.X.; Dai, W.X.; Zhai, S.X.; Lin, J. Nanocomposite Proton Exchange Membranes Incorporating Phosphotungstic Acid Anchored on Imidazole-Functionalized Halloysite Nanotubes. J. Electrochem. Soc. 2018, 165, F951–F958. [Google Scholar] [CrossRef]
  17. He, S.J.; Dai, W.X.; Yang, W.; Liu, S.X.; Bian, X.M.; Zhang, C.; Lin, J. Nanocomposite proton exchange membranes based on phosphotungstic acid immobilized by polydopamine-coated halloysite nanotubes. Polym. Test. 2019, 73, 242–249. [Google Scholar] [CrossRef]
  18. Dong, C.; Wang, Q.; Cong, C.; Meng, X.; Zhou, Q. Influence of alkaline 2D carbon nitride nanosheets as fillers for anchoring HPW and improving conductivity of SPEEK nanocomposite membranes. Int. J. Hydrog. Energy 2017, 42, 10317–10328. [Google Scholar] [CrossRef]
  19. Zhang, B.; Cao, Y.; Li, Z.; Wu, H.; Yin, Y.; Cao, L.; He, X.; Jiang, Z. Proton exchange nanohybrid membranes with high phosphotungstic acid loading within metal-organic frameworks for PEMFC applications. Electrochim. Acta 2017, 240, 186–194. [Google Scholar] [CrossRef]
  20. Bose, A.B.; Gopu, S.; Li, W. Enhancement of proton exchange membrane fuel cells performance at elevated temperatures and lower humidities by incorporating immobilized phosphotungstic acid in electrodes. J. Power Sources 2014, 263, 217–222. [Google Scholar] [CrossRef]
  21. He, S.J.; Lin, Y.K.; Wei, Z.; Zhang, L.Q.; Lin, J.; Nazarenko, S. Solvent-free Fabrication of Proton Conducting Membranes Based on Commercial Elastomers. Polym. Adv. Technol. 2015, 26, 300–307. [Google Scholar] [CrossRef]
  22. Liu, X.; He, S.J.; Shi, Z.Z.; Zhang, L.Q.; Lin, J. Effect of residual casting solvent content on the structure and properties of sulfonated poly(ether ether ketone) membranes. J. Membr. Sci. 2015, 492, 48–57. [Google Scholar] [CrossRef]
  23. Inan, T.Y.; Dogan, H.; Unveren, E.E.; Eker, E. Sulfonated PEEK and fluorinated polymer based blends for fuel cell applications: Investigation of the effect of type and molecular weight of the fluorinated polymers on the membrane’s properties. Int. J. Hydrog. Energy 2010, 35, 12038–12053. [Google Scholar] [CrossRef]
  24. Lin, D.; Yan, X.; He, G.; Wu, X.; Hu, Z.; Wang, Y. SPEEK proton exchange membranes modified with silica sulfuric acid nanoparticles. Int. J. Hydrog. Energy 2012, 37, 11853–11861. [Google Scholar]
  25. Tsai, J.C.; Cheng, H.P.; Kuo, J.F.; Huang, Y.H.; Chen, C.Y. Blended Nafion®/SPEEK direct methanol fuel cell membranes for reduced methanol permeability. J. Power Sources 2009, 189, 958–965. [Google Scholar] [CrossRef]
  26. Martos, A.M.; Biasizzo, M.; Trotta, F.; del Río, C.; Várez, A.; Levenfeld, B. Synthesis and characterization of sulfonated PEEK-WC-PES copolymers for fuel cell proton exchange membrane application. Eur. Polym. J. 2017, 93, 390–402. [Google Scholar] [CrossRef]
  27. Kreuer, K.D. Proton conductivity: Materials and applications. Chem. Mater. 1996, 8, 610–641. [Google Scholar] [CrossRef]
  28. Roudgar, A.; Narasimachary, S.P.; Eikerling, M. Hydrated Arrays of Acidic Surface Groups as Model Systems for Interfacial Structure and Mechanisms in PEMs. J. Phys. Chem. B 2006, 110, 20469–20477. [Google Scholar] [CrossRef]
  29. Kreuer, K.D. On the development of proton conducting polymer membranes for hydrogen and methanol fuel cells. J. Membr. Sci. 2001, 185, 29–39. [Google Scholar] [CrossRef]
  30. Kreuer, K.D. On the development of proton conducting materials for technological applications. Solid State Ion. 1997, 97, 1–15. [Google Scholar] [CrossRef]
  31. Colomban, P.; Novak, A. Proton conductors: Classification and conductivity. In Proton Conductors: Solids, Membranes and Gels-Materials and Devices; Colomban, P., Ed.; Cambridge University Press: Cambridge, UK, 1992; pp. 38–60. [Google Scholar]
Figure 1. Structural formulae of (a) sulfonated poly(ether ether ketone) (SPEEK) and (b) sodium dodecyl benzene sulfonate (SDBS).
Figure 1. Structural formulae of (a) sulfonated poly(ether ether ketone) (SPEEK) and (b) sodium dodecyl benzene sulfonate (SDBS).
Polymers 11 00203 g001
Figure 2. SEM images of (a) a SPEEK membrane and SPEEK/SDBS membranes with SDBS contents of (b) 2 wt %, (c) 4 wt %, (d) 10 wt %, (e) 15 wt %, and (f) 20 wt %.
Figure 2. SEM images of (a) a SPEEK membrane and SPEEK/SDBS membranes with SDBS contents of (b) 2 wt %, (c) 4 wt %, (d) 10 wt %, (e) 15 wt %, and (f) 20 wt %.
Polymers 11 00203 g002
Figure 3. Ion exchange capacities (IECs) of SPEEK/SDBS membranes with various SDBS contents.
Figure 3. Ion exchange capacities (IECs) of SPEEK/SDBS membranes with various SDBS contents.
Polymers 11 00203 g003
Figure 4. Proton conductivity and water uptake of SPEEK/SDBS membranes (solid symbols) with various SDBS contents and a SPEEK membrane with a degree of sulfonation (DS) of 73% (open symbols)
Figure 4. Proton conductivity and water uptake of SPEEK/SDBS membranes (solid symbols) with various SDBS contents and a SPEEK membrane with a degree of sulfonation (DS) of 73% (open symbols)
Polymers 11 00203 g004
Figure 5. Arrhenius plots of proton conductivity for a SPEEK membrane and SPEEK/SDBS membranes with SDBS contents of 2 wt %, 4 wt %, and 10 wt % as a function of temperature.
Figure 5. Arrhenius plots of proton conductivity for a SPEEK membrane and SPEEK/SDBS membranes with SDBS contents of 2 wt %, 4 wt %, and 10 wt % as a function of temperature.
Polymers 11 00203 g005
Figure 6. Schematic diagram of proton transport mechanisms in the SPEEK/SDBS membranes.
Figure 6. Schematic diagram of proton transport mechanisms in the SPEEK/SDBS membranes.
Polymers 11 00203 g006
Figure 7. Proton conductivity of the SPEEK/SDBS-10 membrane as a function of immersion time in deionized (DI) water.
Figure 7. Proton conductivity of the SPEEK/SDBS-10 membrane as a function of immersion time in deionized (DI) water.
Polymers 11 00203 g007
Figure 8. Stress–strain curves of a SPEEK membrane and SPEEK/SDBS membranes with SDBS contents of 2 wt %, 4 wt %, and 10 wt %.
Figure 8. Stress–strain curves of a SPEEK membrane and SPEEK/SDBS membranes with SDBS contents of 2 wt %, 4 wt %, and 10 wt %.
Polymers 11 00203 g008
Table 1. Mechanical properties of SPEEK/SDBS membranes.
Table 1. Mechanical properties of SPEEK/SDBS membranes.
PerformanceElastic Modulus (GPa)Yield Strength (MPa)Tensile Strength (MPa)Elongation at Break (%)
SPEEK1.7263.763.0110
SPEEK/SDBS-21.7056.652.885
SPEEK/SDBS-41.4245.444.958
SPEEK/SDBS-100.92-37.929

Share and Cite

MDPI and ACS Style

Zhai, S.; Dai, W.; Lin, J.; He, S.; Zhang, B.; Chen, L. Enhanced Proton Conductivity in Sulfonated Poly(ether ether ketone) Membranes by Incorporating Sodium Dodecyl Benzene Sulfonate. Polymers 2019, 11, 203. https://doi.org/10.3390/polym11020203

AMA Style

Zhai S, Dai W, Lin J, He S, Zhang B, Chen L. Enhanced Proton Conductivity in Sulfonated Poly(ether ether ketone) Membranes by Incorporating Sodium Dodecyl Benzene Sulfonate. Polymers. 2019; 11(2):203. https://doi.org/10.3390/polym11020203

Chicago/Turabian Style

Zhai, Shaoxiong, Wenxu Dai, Jun Lin, Shaojian He, Bing Zhang, and Lin Chen. 2019. "Enhanced Proton Conductivity in Sulfonated Poly(ether ether ketone) Membranes by Incorporating Sodium Dodecyl Benzene Sulfonate" Polymers 11, no. 2: 203. https://doi.org/10.3390/polym11020203

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop