Next Article in Journal
Fatigue Life Prediction for Carbon-SMC and Carbon-FRP by Considering Elastic Modulus Degradation
Next Article in Special Issue
Modeling and Simulations of the Sulfur Infiltration in Activated Carbon Fabrics during Composite Cathode Fabrication for Lithium-Sulfur Batteries
Previous Article in Journal
Dielectric Constant Enhancement with Low Dielectric Loss Growth in Graphene Oxide/Mica/Polypropylene Composites
Previous Article in Special Issue
Interactions of Cd2+, Co2+ and MoO42− Ions with Crushed Concrete Fines
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

A Lamination Model for Pressure-Assisted Sintering of Multilayered Porous Structures

1
Department of Mechanical Engineering, University of Maine, Orono, ME 04469, USA
2
Manufacturing Science Division, Oak Ridge National Laboratory, Oak Ridge, TN 37830, USA
*
Author to whom correspondence should be addressed.
J. Compos. Sci. 2021, 5(2), 53; https://doi.org/10.3390/jcs5020053
Submission received: 14 January 2021 / Revised: 2 February 2021 / Accepted: 3 February 2021 / Published: 9 February 2021
(This article belongs to the Special Issue Feature Papers in Journal of Composites Science in 2020)

Abstract

:
This work describes a lamination model for pressure-assisted sintering of thin, multilayered, and porous structures based on the linear viscous constitutive theory of sintering and the classical laminated plate theory of continuum mechanics. A constant out-of-plane normal stress is assumed in the constitutive relation. The lamination relations between the force/moment resultants and the strain/curvature rates are presented. Numerical simulations were performed for a symmetric tri-layer laminate consisting of a 10% gadolinia doped ceria (Ce0.9Gd0.1O1.95-δ) composite structure, where porous layers were adhered to the top and bottom of a denser layer under uniaxially-applied pressures and the sinter forging conditions. The numerical results show that, compared with free sintering, the applied pressure can significantly reduce the sintering time required to achieve given layer thicknesses and porosities. Unlike free sintering, which results in a monotonic decrease of the laminate in-plane dimension, pressure-assisted sintering may produce an in-plane dimension increase or decrease, depending on the applied pressure and sintering time. Finally, the individual layers in the laminate exhibit different stress characteristics under pressure-assisted sintering.

1. Introduction

Ceramic-based multilayers are of importance for a wide range of applications, including solid oxide fuel cells, batteries, capacitors, sensors, thermo-electrics, and windows [1,2,3,4,5]. Integrated printing and sintering is a new processing technology for manufacturing multilayered ceramic materials. This integrated method is a fast and cost-effective way to enhance the functional and mechanical properties of materials compared with traditional material processing approaches, for example, vapor deposition. However, differential densifications in the individual layers during sintering will influence sintering kinetics, and can cause stresses resulting in defects, cracks, and macro-structural distortion. Modelling and understanding sintering kinetics, as well as the shrinkage and distortion, is thus critically important for the efficient manufacturing of multilayers and their applications to provide quality parts with limited defects [6,7,8].
In processing multilayers with powder-based materials, the sintering of these materials is typically done once the material is printed, casted, or pressed [9,10,11]. When sintering thin ceramic material on top of another material of greater or lesser density, or even on a substrate, the sintering behavior of the multilayers is much different from free sintering of a part, because the strain rates, or rate of densification, of the two materials are different, causing one layer to peel off the other or the warping of the multilayer as a whole [12]. The phenomena that causes this distortion is known as constrained sintering [8], and continuum mechanics models have been developed to understand the difference in stress states of the material as a macroscopic viscoelastic body [13,14]. Pressure-assisted sintering has been used to lower the sintering time and temperature, and to minimize grain growth [15]. The reason for these kinetic enhancements is from enhanced diffusion from the creep mechanisms, such as Coble creep and Nabarro-Herring creep, resulting in mechanisms like grain boundary sliding [16,17]. Cramer et al. [18] assessed the constraints and strain rates with pressure-assisted sintering on porous oxide bodies with controlled porosity. Continuum-based models for free and pressure-assisted sintering of multilayered ceramic structures are essential to the design of geometries or configurations in which no warping or distortion occurs, except for the inherent uniform shrinkage.
There has also been some work with 3D printed and tape-casted parts utilizing multilayer and multi-material approaches for making bulk structures [19,20,21,22,23], but a better understanding of the sintering and processing with and without an applied mechanical load is needed to achieve the best densities and properties. Fundamentally, 3D printing of materials needing sintering may have the same constraints as multilayers with different densities because of gaps, defects, and layering effects [22,23], but the focus of this research does not discuss this further.
In modeling shrinkage and distortion behavior of sintered multilayered porous structures, reasonable assumptions on the strain distribution through the thickness can often be used without compromising the accuracy of the models. An assumption of a uniform strain rate through the thickness of each layer was used by Chang et al. [6], Chiang et al. [7], and Ni et al. [24]. The uniform strain rate assumption may be used for a laminate consisting of extremely thin layers or a laminate that is symmetric about its geometrical mid-plane. For general multilayered structures, better accuracy may be achieved using a linear strain distribution assumption, as suggested by Kanters et al. [25], who simulated densification and warpage during sintering of a bi-layered nanocrystalline zirconia structure. Most recently, Molla et al. [26] modeled shrinkage and distortion of a bi-layered structure using a continuum, linear viscous theory of sintering applied to Ce0.9Gd0.1O(1.95−δ) (CGO). Olevsky et al. [27] and Ni et al. [28] developed a constitutive model for free sintering of multilayered porous structures, and applied the model to sintering of bi-layered CGO structures, showing how all of the parameters and state variables effect the stress, porosity, and distortion. They also developed some conditions for tri-layered structures, but the pressure effects were not considered. Besides structural mechanics-based models as reviewed above, Molla et al. [29] studied shape distortion of bilayers with different densities using a multiscale model. Shabana et al. [30] modeled stress evolutions in a metal–ceramic functionally graded material during free sintering using a viscoplastic constitutive model. We point out that pressure-assisted sintering of multilayered structures was not considered in the studies of Olevsky and co-workers [26,27,28,29]. Continuum-based models for pressure-assisted sintering of multilayers have not been available in the literature to the best knowledge of the authors.
The purpose of this work is to present a lamination model for pressure-assisted sintering of thin multilayered porous structures. The model is based on the linear viscous constitutive theory of sintering [31] and a laminated plate theory of continuum mechanics [32]. The remainder of the paper is organized as follows. Section 2 reviews the constitutive relations of a linear viscous theory of sintering [31]. In Section 3, the basic equations for sintering of multilayered structures are derived based on the Kirchhoff hypotheses of classical laminated plate theory, considering the applied out-of-plane pressure. In Section 4, the lamination model is applied to pressure-assisted sintering of a symmetric, tri-layer structure. A sinter forging condition is assumed, i.e., the tri-layer structure is not confined in the in-plane directions. Numerical examples are given in Section 5 for a CGO_P/CGO_D/CGO_P tri-layer laminate, where CGO_P is the porous layer and CGO_D is a denser layer. Finally, concluding remarks and discussions of the limitations of the lamination model are provided in Section 6.

2. Constitutive Equations of Sintering

In this work, we employ the following linear viscous theory of sintering [31]:
σ i j = 2 η 0 ϕ ε ˙ i j + ψ 1 3 ϕ ε ˙ k k δ i j + P L δ i j
where σij is the stresses, ε ˙ i j is the strain rates, PL is the effective sintering stress, δij is the Kronecker delta, η0 is the shear viscosity of the fully dense material, φ is the normalized shear viscosity, ψ is the normalized bulk viscosity, the indices i, j, and k have the range of 1 to 3 (or x, y, and z), and a repeated index implies summation over the range of the index. According to Olevsky [31], φ, ψ, and PL are related to the porosity by:
ϕ = ( 1 θ ) 2 , ψ = 2 ( 1 θ ) 3 3 θ , P L = 3 α 2 G ( 1 θ ) 2
where θ is the porosity of the body being sintered, G is the grain size (average particle radius), and α is the surface energy per unit area (surface energy density). The evolution equation of porosity is based on the continuity equation, and is given by:
θ ˙ 1 θ = ε ˙ k k
where the superimposed dot denotes the derivative with respect to time.
The total strain rate is the sum of the stress-induced creep strain rate and the free sintering strain rate, i.e.,
ε ˙ i j = ε ˙ i j c + ε ˙ f δ i j
where ε ˙ i j c is the creep strain rates, and ε ˙ f is the free linear sintering strain rate given by [31].
ε ˙ f = P L 6 η 0 ψ
Substituting Equations (4) and (5) into Equation (1) yields:
σ i j = 2 η 0 ϕ ε ˙ i j c + ψ 1 3 ϕ ε ˙ k k c δ i j

3. A Lamination Model for Pressure-Assisted Sintering of Multilayered Porous Structures

Consider an N-layered porous structure, as shown in Figure 1, where hi (i = 1, 2, …, N) is the thickness of the ith layer, and H is the total thickness of the laminate, i.e., H = h1 + h2 + … + hN. The rectangular coordinates (x, y, z) are selected so that the x–y plane is the mid-plane of the laminate and z is normal to the laminate plane.

3.1. Stress-Strain Rate Relation

For thin multilayered structures, the normal stress in the z direction may be assumed as the applied pressure (a constant) in pressure-assisted sintering, and the shear stresses associated with the z direction may be assumed as zero, i.e., σ z = σ z 0 ( σ z 0 = 0 for free sintering, as in Olevsky et al. [27]), and σxz = σyz = 0. Now Equation (6) reduces to:
σ x x = 2 η 0 ϕ ψ + 2 3 ϕ 2 ψ + 1 3 ϕ ε ˙ x x c + ψ 1 3 ϕ ε ˙ y y c + ψ 1 3 ϕ ψ + 2 3 ϕ σ z 0 , σ y y = 2 η 0 ϕ ψ + 2 3 ϕ 2 ψ + 1 3 ϕ ε ˙ y y c + ψ 1 3 ϕ ε ˙ x x c + ψ 1 3 ϕ ψ + 2 3 ϕ σ z 0 , σ x y = 2 η 0 ϕ ε ˙ x y c = 2 η 0 ϕ ε ˙ x y
The inverse form of the above relation is:
ε ˙ x x c = 1 6 η 0 ϕ ψ 2 ψ + 1 3 ϕ σ x x ψ 1 3 ϕ σ y y + ψ 1 3 ϕ 1 3 ψ 1 2 ψ 1 3 ϕ ψ + 2 3 ϕ σ z 0 ϕ η 0 , ε ˙ y y c = 1 6 η 0 ϕ ψ 2 ψ + 1 3 ϕ σ y y ψ 1 3 ϕ σ x x + ψ 1 3 ϕ 1 3 ψ 1 2 ψ 1 3 ϕ ψ + 2 3 ϕ σ z 0 ϕ η 0 , ε ˙ x y c = ε ˙ x y = σ x y 2 η 0 ϕ
The normal creep strain rate in the thickness direction of the multilayered structures can be derived as follows:
  ε ˙ z z c = 1 6 η 0 ϕ ψ ψ 1 3 ϕ ( σ x x + σ y y ) + 1 2 + ψ 1 3 ϕ 2 1 3 ψ ϕ σ z 0 / η 0 ψ + 2 3 ϕ = 1 ψ + 2 3 ϕ ψ 1 3 ϕ ( ε ˙ x x c + ε ˙ y y c ) + σ z 0 / ( 2 η 0 ) ψ + 2 3 ϕ
The relations in Equations (7)–(9) are applicable to individual layers in the laminate, and the layers may have different properties.

3.2. Strain Rates

The Kirchhoff hypotheses of the classical plate theory may be used for sintering of thin multilayered structures [26,27]. Based on the Kirchhoff hypotheses [32], the in-plane strain rates in the laminate can be expressed as:
ε ˙ x x = ε ˙ x 0 ( x , y ) + z κ ˙ x 0 ( x , y ) , ε ˙ y y = ε ˙ y 0 ( x , y ) + z κ ˙ y 0 ( x , y ) , γ ˙ x y = 2 ε ˙ x y ( x , y ) = γ ˙ x y 0 ( x , y ) + z κ ˙ x y 0 ( x , y )
where ε ˙ x 0 , ε ˙ y 0 , and γ ˙ x y 0 are the strain rates of the geometrical mid-plane (z = 0), and κ ˙ x 0 , κ ˙ y 0 , and κ ˙ x y 0 are the curvature rates of the mid-plane. The creep strain rates are given by:
ε ˙ x x c = ε ˙ x 0 + z κ ˙ x 0 ε ˙ f , ε ˙ y y c = ε ˙ y 0 + z κ ˙ y 0 ε ˙ f , γ ˙ x y c = γ ˙ x y = γ ˙ x y 0 + z κ ˙ x y 0
Substituting the creep strain rates from Equation (11) into Equation (7), we have the following stress expressions:
σ x x = 2 η 0 ϕ ψ + 2 3 ϕ 2 ψ + 1 3 ϕ ( ε ˙ x 0 + z κ ˙ x 0 ) + ψ 1 3 ϕ ( ε ˙ y 0 + z κ ˙ y 0 ) 3 ψ ε ˙ f + ψ 1 3 ϕ ψ + 2 3 ϕ σ z 0 σ y y = 2 η 0 ϕ ψ + 2 3 ϕ 2 ψ + 1 3 ϕ ( ε ˙ y 0 + z κ ˙ y 0 ) + ψ 1 3 ϕ ( ε ˙ x 0 + z κ ˙ x 0 ) 3 ψ ε ˙ f + ψ 1 3 ϕ ψ + 2 3 ϕ σ z 0 σ x y = η 0 ϕ γ ˙ x y 0 + z κ ˙ x y 0
The above expressions are valid for stresses in every layer of the laminate.

3.3. Force and Moment Resultants

Define the following force and moment resultants [32] as:
N x = H / 2 H / 2 σ x x d z , N y = H / 2 H / 2 σ y y d z , N x y = H / 2 H / 2 σ x y d z , M x = H / 2 H / 2 σ x x z d z , M y = H / 2 H / 2 σ y y z d z , M x y = H / 2 H / 2 σ x y z d z
Substituting the stresses in Equation (12) into the above equation, we obtain the following relations between the force/moment resultants and the strain/curvature rates:
N x = A 11 ε ˙ x 0 + A 12 ε ˙ y 0 + B 11 κ ˙ x 0 + B 12 κ ˙ y 0 N f + N z 0 N y = A 12 ε ˙ x 0 + A 11 ε ˙ y 0 + B 12 κ ˙ x 0 + B 11 κ ˙ y 0 N f + N z 0 N x y = A 66 γ ˙ x y 0 + B 66 κ ˙ x y 0
and
M x = B 11 ε ˙ x 0 + B 12 ε ˙ y 0 + D 11 κ ˙ x 0 + D 12 κ ˙ y 0 M f + M z 0 M y = B 12 ε ˙ x 0 + B 11 ε ˙ y 0 + D 12 κ ˙ x 0 + D 11 κ ˙ y 0 M f + M z 0 M x y = B 66 γ ˙ x y 0 + D 66 κ ˙ x y 0
where
A 11 = i = 1 N 2 η 0 i ϕ i ψ i + 2 3 ϕ i 2 ψ i + 1 3 ϕ i ( z i z i 1 ) , A 12 = i = 1 N 2 η 0 i ϕ i ψ i + 2 3 ϕ i ψ i 1 3 ϕ i ( z i z i 1 ) , A 66 = i = 1 N η 0 i ϕ i ( z i z i 1 )
B 11 = i = 1 N 2 η 0 i ϕ i ψ i + 2 3 ϕ i 2 ψ i + 1 3 ϕ i 1 2 ( z i 2 z i 1 2 ) , B 12 = i = 1 N 2 η 0 i ϕ i ψ i + 2 3 ϕ i ψ i 1 3 ϕ i 1 2 ( z i 2 z i 1 2 ) , B 66 = i = 1 N η 0 i ϕ i 1 2 ( z i 2 z i 1 2 )  
D 11 = i = 1 N 2 η 0 i ϕ i ψ i + 2 3 ϕ i 2 ψ i + 1 3 ϕ i 1 3 ( z i 3 z i 1 3 ) , D 12 = i = 1 N 2 η 0 i ϕ i ψ i + 2 3 ϕ i ψ i 1 3 ϕ i 1 3 ( z i 3 z i 1 3 ) , D 66 = i = 1 N η 0 i ϕ i 1 3 ( z i 3 z i 1 3 )  
and
N f = i = 1 N 6 η 0 i ϕ i ψ i ε ˙ f i ψ i + 2 3 ϕ i ( z i z i 1 ) , M f = i = 1 N 6 η 0 i ϕ i ψ i ε ˙ f i ψ i + 2 3 ϕ i 1 2 ( z i 2 z i 1 2 ) , N z 0 = σ z 0 i = 1 N ψ i 1 3 ϕ i ψ i + 2 3 ϕ i ( z i z i 1 ) , M z 0 = σ z 0 i = 1 N ψ i 1 3 ϕ i ψ i + 2 3 ϕ i 1 2 ( z i 2 z i 1 2 )
In Equations (16a)–(17):
z i = H 2 + j = 1 i h j   ( i = 1 , 2 , , N ) ,   z 0 = H 2 = 1 2 j = 1 N h j
The above relations between the force/moment resultants and the strain/curvature rates are an extension of those introduced in Olevsky et al. [27] for free sintering with iso-stretch in the laminate plane, i.e., ε ˙ x = ε ˙ y . Moreover, the N z 0 and M z 0 terms are zero for free sintering.

4. Pressure-Assisted Sintering of a Symmetric Tri-Layer Structure

In this section, we apply the lamination model presented in Section 3 to pressure-assisted sintering of a symmetric tri-layer structure. A sinter forging condition is assumed, i.e., the tri-layer structure is not confined in the in-plane directions. Free sintering of this laminate was studied by Olevsky et al. [27] and Ni et al. [28], but their stress and stress resultants need to be developed further. The outside layers, i.e., layer #1 and #3, have the same material properties and thickness, i.e., η01 = η03, α1 = α3, G1 = G3, φ1 = φ3, ψ1 = ψ3, and h1 = h3. Bending and twisting thus do not occur due to the symmetry, i.e., κ ˙ x 0 = κ ˙ y 0 = κ ˙ x y 0 = 0 . Moreover, B11 = B12 = B66 = 0 and M f = M z 0 = 0 in Equations (14)–(17). For sinter forging with the applied pressure in the z direction, all stress resultants in Equation (14) are zero. The stresses in individual layers, however, do exist because of the material mismatch between the outside and middle layers. Because no shear deformation exists, the lamination Equation (14) now reduces to:
( A 11 + A 12 ) ε ˙ 0 = N f N z 0
where ε ˙ 0 is the normal strain rate in the x and y directions, i.e.,
ε ˙ 0 = ε ˙ x 0 = ε ˙ y 0
and
A 11 + A 12 = 2 6 η 01 ϕ 1 ψ 1 ψ 1 + 2 3 ϕ 1 h 1 + 6 η 02 ϕ 2 ψ 2 ψ 2 + 2 3 ϕ 2 h 2 , N f = 2 6 η 01 ϕ 1 ψ 1 ε ˙ f 1 ψ 1 + 2 3 ϕ 1 h 1 + 6 η 02 ϕ 2 ψ 2 ε ˙ f 2 ψ 2 + 2 3 ϕ 2 h 2 , N z 0 = σ z 0 2 ψ 1 1 3 ϕ 1 ψ 1 + 2 3 ϕ 1 h 1 + ψ 2 1 3 ϕ 2 ψ 2 + 2 3 ϕ 2 h 2
Submitting Equation (21) into Equation (19) yields the in-plane strain rate as follows:
ε ˙ 0 = 2 ϕ 1 ψ 1 ψ 2 + 2 3 ϕ 2 ε ˙ f 1 + ( η 02 / η 01 ) ϕ 2 ψ 2 ψ 1 + 2 3 ϕ 1 ε ˙ f 2 ( h 2 / h 1 ) 2 ϕ 1 ψ 1 ψ 2 + 2 3 ϕ 2 + ( η 02 / η 01 ) ϕ 2 ψ 2 ψ 1 + 2 3 ϕ 1 ( h 2 / h 1 ) σ z 0 6 η 01 2 ψ 1 1 3 ϕ 1 ψ 1 + 2 3 ϕ 1 + ψ 2 1 3 ϕ 2 ψ 2 + 2 3 ϕ 2 h 2 h 1 / 2 ϕ 1 ψ 1 ψ 1 + 2 3 ϕ 1 + ( η 02 / η 01 ) ϕ 2 ψ 2 ψ 2 + 2 3 ϕ 2 h 2 h 1
which equals L ˙ / L , i.e., the in-plane dimension kinetics, in which L is an in-plane dimension.
The governing equations for the evolution of porosities in the individual layers can be obtained from Equations (2), (3), (5), (8), (9), (11), and (20) as follows:
θ ˙ 1 1 θ 1 = 2 ε ˙ 0 ϕ 1 ψ 1 + 2 3 ϕ 1 9 θ 1 8 ( 1 θ 1 ) α 1 G 1 η 01 + σ z 0 / ( 2 η 01 ) ψ 1 + 2 3 ϕ 1 , θ ˙ 2 1 θ 2 = 2 ε ˙ 0 ϕ 2 ψ 2 + 2 3 ϕ 2 9 θ 2 8 ( 1 θ 2 ) α 2 G 2 η 02 + σ z 0 / ( 2 η 02 ) ψ 2 + 2 3 ϕ 2
The governing equations for the thickness shrinkage rates of the individual layers can be obtained from Equations (4), (9), (11), and (20), with the results:
h ˙ 1 h 1 = ε ˙ z 1 = ε ˙ f 1 1 ψ 1 + 2 3 ϕ 1 ψ 1 1 3 ϕ 1 ( 2 ε ˙ 0 2 ε ˙ f 1 ) + σ z 0 / ( 2 η 01 ) ψ 1 + 2 3 ϕ 1 , h ˙ 2 h 2 = ε ˙ z 2 = ε ˙ f 2 1 ψ 2 + 2 3 ϕ 2 ψ 2 1 3 ϕ 2 ( 2 ε ˙ 0 2 ε ˙ f 2 ) + σ z 0 / ( 2 η 02 ) ψ 2 + 2 3 ϕ 2
Equations (23) and (24) are four simultaneous first-order differential equations to determine the evolutions of thicknesses and porosities h1, h2, θ1, and θ2 with ε ˙ 0 given in Equation (22). Moreover, the free sintering strains ε ˙ f i are given by:
ε ˙ f i   = 3 θ i 8 ( 1 θ i ) α i G i η 0 i , i = 1 , 2
Following Olevsky [31], we use the following dimensionless thicknesses and specific dimensionless sintering time:
h 1 * = h 1 h 01 , h 2 * = h 2 h 02 ,   τ s = 3 0 t α 1 G 1 η 01 d t
where h01 and h02 are the initial thicknesses. With the above dimensionless quantities, Equations (23) and (24) take the following normalized forms:
d θ 1 d τ s = 2 ε ˙ 0 G 1 η 01 3 α 1 ϕ 1 ( 1 θ 1 ) ψ 1 + 2 3 ϕ 1 3 θ 1 8 + ( 1 θ 1 ) ψ 1 + 2 3 ϕ 1 σ z 0 2 η 01 G 1 η 01 3 α 1 , d θ 2 d τ s = 2 ε ˙ 0 G 1 η 01 3 α 1 ϕ 2 ( 1 θ 2 ) ψ 2 + 2 3 ϕ 2 3 θ 2 8 G 1 η 01 G 2 η 02 α 2 α 1 + ( 1 θ 2 ) ψ 2 + 2 3 ϕ 2 σ z 0 2 η 02 G 1 η 01 3 α 1
d h 1 * d τ s = θ 1 8 ( 1 θ 1 ) h 1 * 2 h 1 * ψ 1 + 2 3 ϕ 1 ψ 1 1 3 ϕ 1 ε ˙ 0 G 1 η 01 3 α 1 + θ 1 8 ( 1 θ 1 ) + h 1 * ψ 1 + 2 3 ϕ 1 σ z 0 2 η 01 G 1 η 01 3 α 1 , d h 2 * d τ s = θ 2 8 ( 1 θ 2 ) α 2 α 1 G 1 η 01 G 2 η 02 h 2 * 2 h 2 * ψ 2 + 2 3 ϕ 2 ψ 2 1 3 ϕ 2 ε ˙ 0 G 1 η 01 3 α 1 + θ 2 8 ( 1 θ 2 ) α 2 α 1 G 1 η 01 G 2 η 02 + h 2 * ψ 2 + 2 3 ϕ 2 σ z 0 2 η 02 G 1 η 01 3 α 1
The initial conditions now are:
θ 1 = θ 01 , τ s = 0 θ 2 = θ 02 , τ s = 0 h 1 * = h 2 * = 1 , τ s = 0
The normalized stresses in each layer can be obtained from Equations (2), (12), and (20) as follows:
σ x 1 P L 1 = σ y 1 P L 1 = 6 ϕ 1 ψ 1 ψ 1 + 2 3 ϕ 1 G 1 η 01 α 1 ε ˙ 0 G 1 η 01 α 1 ε ˙ f 1 2 3 ( 1 θ 1 ) 2 + ψ 1 1 3 ϕ 1 ψ 1 + 2 3 ϕ 1 2 G 1 σ z 0 / α 1 3 ( 1 θ 1 ) 2 , σ x 2 P L 1 = σ y 2 P L 1 = 2 3 ( 1 θ 1 ) 2 6 ( η 02 / η 01 ) ϕ 2 ψ 2 ψ 2 + 2 3 ϕ 2 G 1 η 01 α 1 ε ˙ 0 G 1 η 01 α 1 ε ˙ f 2 + ψ 2 1 3 ϕ 2 ψ 2 + 2 3 ϕ 2 2 G 1 σ z 0 / α 1 3 ( 1 θ 1 ) 2

5. Numerical Results

This section presents numerical results of porosity evolution, thickness shrinkage, in-plane dimension change, and stresses for sinter forging of a symmetric CGO_P/CGO_D/CGO_P laminate, where CGO stands for gadolinium 10% doped ceria Ce0.9Gd0.1O1.95−δ. CGO_P and CGO_D stand for a porous and a dense (less porous) CGO, respectively. Ni et al. [28] manufactured a CGO_P/CGO_D/CGO_P laminate under free sintering without applying pressures. The outside layers (i.e., layers 1 and 3, CGO_P) and mid-layer (i.e., layer 2, CGO_D) are the same material under the fully dense condition. Hence, we assume that they have the same material properties, i.e., the same shear viscosity of fully dense material η0, and the same surface energy per unit area α. Moreover, we assume they also have the same grain size, G. Therefore, the property ratios are η0201 = 1, α21 = 1, and G2/G1 = 1. Following Ni et al. [28], the initial porosities are assumed as θ01 = 0.65 and θ02 = 0.45, respectively, and the initial thicknesses are h01 = h03 = 0.4 mm and h02 = 0.03 mm, respectively. These initial thicknesses correspond to the thicknesses after a debinder cycle before sintering [28]. Grain growth is not considered. The grain sizes are G1 = 1.0 μm and G2 = 1.0 μm for the CGO_P and CGO_D, respectively. The surface energies per unit area are α1 = 1.0 J/m2 and α2 = 1.0 J/m2 for the CGO_P and CGO_D, respectively.
Figure 2a,b shows the porosity evolutions in the CGO_P (layers 1 and 3) and CGO_D (layer 2) layers, respectively. Two applied axial pressures are considered, i.e., P = σ z 0 = 1 MPa and 5 MPa. The porosities monotonically decrease as time evolves. The porosity is significantly reduced by the applied pressure at a given sintering time. The middle CGO_D layer becomes fully dense (i.e., zero porosity) at specific sintering times of 2.75, 2.1, and 1.05 under free sintering, with 1 MPa of pressure and 5 MPa of pressure, respectively. The porosity of the outside CGO_P layers reduces to 0.15, 0.094, and 0.026 at a specific sintering time of 3.0 under free sintering, with 1 MPa of pressure and 5 MPa of pressure, respectively.
The shrinkages of normalized thicknesses are shown in Figure 3a,b. The thicknesses of both layers decrease monotonically with time, with the rate of reduction gradually leveling off. The normalized thickness of the middle CGO_D layer decreases to about 0.94, 0.658, and 0.277 at a specific sintering time of 3 under free sintering, with 1 MPa of pressure and 5 MPa of pressure, respectively. The corresponding dimensional thicknesses are 0.028 mm, 0.0197, and 0.0083 mm, respectively. At the same time, the normalized thicknesses of the outside CGO_P layers decrease to 0.891, 0.594, and 0.221, respectively, and the corresponding dimensional thicknesses are 0.356 mm, 0.238 mm, and 0.0884 mm, respectively. The values for free sintering compare to the experimental data of 0.02 mm for the CGO_D layer and 0.28 mm for the CGO_P layers, respectively [28].
Figure 4 shows the kinetics of the in-plane dimension of the laminate. All three layers are assumed to deform together in the lamination model. The normalized dimension shrinks under free sintering, and the dimension reduces to about 0.824 at a specific sintering time of 3.0. The test result of Ni et al. [28] is about 0.7. The trends of kinetics of dimensional shrinkages and porosities are consistent with the experimental results of Ni et al. [28]. A number of factors may contribute to the difference between the theoretical predictions of this work and the experimental results of Ni et al. [28]. For example, grain growth may affect porosity and hence geometrical dimensions. Furthermore, the linear viscous sintering theory may not exactly describe the material behavior under sintering. For pressure-assisted sintering, the in-plane dimension monotonically increases with time under a 5 MPa pressure, and reaches 2.64 at a specific sintering time of 3. Under a pressure of 1 MPa, the normalized in-plane dimension initially decreases with time, reaches a minimum of 0.988 at a specific sintering time of 0.3, and then increases with time. The increase in the in-plane dimension under sinter forging is due to the uniaxial pressure in the thickness direction.
Figure 5a,b shows the normalized stresses developed in the CGO_P (layers 1 and 3) and CGO_D (layer 2) layers, respectively. Stresses developed in the individual layers because of a porosity mismatch, which results in differential free sintering strain rates. The CGO_P and CGO_D layers respond differently under free and pressure-assisted sintering. Under free sintering, the in-plane dimension shrinks, as shown in Figure 4. Hence, the outside CGO_P layers are subjected to tensile stress, which decreases with time. Compressive stress is developed in the middle CGO_D layer, and its magnitude also decreases with time. The magnitude of the stress in the CGO_D layer is significantly larger than that in the CGO_P layers, because the CGO_D layer is much thinner than the CGO_P layers as assumed. For sintering under the 1 MPa of uniaxial pressure, the individual layers respond similarly, although, generally, the magnitudes of the stresses become smaller. For sintering under the 5 MPa uniaxial pressure, however, the outside CGO_P layers are mostly subjected to compressive stress, and the middle CGO_D layer is mostly subjected to tensile stress.
A sensitivity analysis is performed to evaluate the dependence of the sintering kinetics on the thickness of the mid CGO_D layer. Figure 6 and Figure 7 show the evolutions of porosity and normalized thickness in the CGO_P (layers 1 and 3) and CGO_D (layer 2) layers, respectively, for a larger initial thickness of the mid layer of h02 = 0.1 mm. Other parameters remain the same as those in Figure 2 and Figure 3. Comparing with the results in Figure 2 and Figure 3, it can be seen that this variation in the mid layer thickness has an insignificant influence on the porosity and normalized thickness evolutions.

6. Concluding Remarks

In this work, we present a continuum lamination model for pressure-assisted sintering of thin, multilayered, and porous structures based on a linear viscous constitutive theory of sintering and the classical lamination theory of plates. The lamination relations satisfied by the strain/curvature rates and force/moment resultants considering the applied out-of-plane pressure are derived. Application of the lamination model to sinter forging of a symmetric, tri-layer CGO_P/CGO_D/CGO_P structure under uniaxial pressure indicates that (i) both the porosities and thicknesses of the individual layers are significantly reduced by the applied pressure at a given sintering time, (ii) whereas the normalized in-plane dimension monotonically decreases with time under free sintering, the in-plane dimension may increase or decrease under sinter forging, depending on the magnitude of the applied pressure and sintering time, and (iii) the individual layers can exhibit complex stress characteristics under pressure-assisted sintering. The applied uniaxial pressure may produce tensile or compressive stress in a given individual layer, depending on the magnitude of the pressure. Finally, for the layered structure modelled here, the mid-layer thickness does not play a significant role in the densification.
This paper only considers sinter forging of multilayered structures under uniaxial pressures. In most pressure-assisted sintering, the in-plane movement of the material is normally constrained, which results in neither a uniaxial pressure nor isostatic pressure condition. The present model will be improved to include the effects of in-plane constraints in a future study. Overall, the lamination model presented in this paper is capable of predicting the effects of applied pressure on sintering kinetics, including evolutions of porosities and thicknesses of the individual layers, and the in-plane dimensions of the structure.

Author Contributions

Conceptualization, Z.-H.J. and C.L.C.; methodology, Z.-H.J.; validation, Z.-H.J. and C.L.C.; formal analysis, Z.-H.J. and C.L.C.; investigation, Z.-H.J. and C.L.C.; data curation, Z.-H.J. and C.L.C.; writing—original draft preparation, Z.-H.J. and C.L.C.; writing—review and editing, Z.-H.J. and C.L.C.; funding acquisition, C.L.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Acknowledgments

C.L.C. acknowledges support by the U.S. Department of Energy, Office of Energy Efficiency and Renewable Energy, Office of Advanced Manufacturing, under contract number DE-AC05-00OR22725.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Tummala, R.R. Ceramic and Glass-Ceramic Packaging in the 1990s. J. Am. Ceram. Soc. 1991, 74, 895–908. [Google Scholar] [CrossRef]
  2. Imanaka, Y. Multilayered Low Temperature Cofired Ceramics (LTCC) Technology; Springer: New York, NY, USA, 2005. [Google Scholar]
  3. Dorey, R.A.; Rocks, S.A.; Dauchy, F.; Wang, D.; Bortolani, F.; Hugo, E. Integrating functional ceramics into microsystems. J. Eur. Ceram. Soc. 2008, 28, 1397–1403. [Google Scholar] [CrossRef]
  4. Singhal, S.C. Solid Oxide Fuel Cells: Status, Challenges and Opportunities. Adv. Sci. Technol. 2006, 45, 1837–1846. [Google Scholar] [CrossRef]
  5. Schwartz, B. Review of multilayer ceramics for microelectronic packaging. J. Phys. Chem. Solids 1984, 45, 1051–1068. [Google Scholar] [CrossRef]
  6. Chang, J.; Guillon, O.; Rödel, J.; Kang, S.-J.L. Characterization of warpage behaviour of Gd-doped ceria/NiO–yttria stabilized zirconia bi-layer samples for solid oxide fuel cell application. J. Power Sources 2008, 185, 759–764. [Google Scholar] [CrossRef]
  7. Chiang, M.-J.; Jean, J.-H.; Lin, S.-C. Effects of green density difference on camber development during the cofiring of a bi-layer glass-based dielectric laminate. Mater. Chem. Phys. 2011, 128, 413–417. [Google Scholar] [CrossRef]
  8. Green, D.J.; Guillon, O.; Rödel, J. Constrained sintering: A delicate balance of scales. J. Eur. Ceram. Soc. 2008, 28, 1451–1466. [Google Scholar] [CrossRef]
  9. Mai, A.; Haanappel, V.A.; Tietz, F.; Stöver, D. Ferrite-based perovskites as cathode materials for anode-supported solid oxide fuel cells: Part II. Influence of the CGO interlayer. Solid State Ionics 2006, 177, 2103–2107. [Google Scholar] [CrossRef]
  10. Tsoga, A.; Gupta, A.; Naoumidis, A.; Skarmoutsos, D.; Nikolopoulos, P. Performance of a double-layer CGO/YSZ electrolyte for solid oxide fuel cells. Ionics 1998, 4, 234–240. [Google Scholar] [CrossRef]
  11. Tzeng, S.-Y.; Jean, J.-H. Stress Development during Constrained Sintering of Alumina/Glass/Alumina Sandwich Structure. J. Am. Ceram. Soc. 2004, 85, 335–340. [Google Scholar] [CrossRef]
  12. Bordia, R.; Raj, R. Sintering Behavior of Ceramic Films Constrained by a Rigid Substrate. J. Am. Ceram. Soc. 1985, 68, 287–292. [Google Scholar] [CrossRef]
  13. Bordia, R.; Scherer, G. On constrained sintering—I. Constitutive model for a sintering body. Acta Met. 1988, 36, 2393–2397. [Google Scholar] [CrossRef]
  14. Li, F.; Pan, J.; Guillon, O.; Cocks, A. Predicting sintering deformation of ceramic film constrained by rigid substrate using ani-sotropic constitutive law. Acta Mater. 2010, 58, 5980–5988. [Google Scholar] [CrossRef]
  15. Guillon, O.; Gonzalez-Julian, J.; Dargatz, B.; Kessel, T.; Schierning, G.; Räthel, J.; Herrmann, M. Field-assisted sintering tech-nology/spark plasma sintering: Mechanisms, materials, and technology developments. Adv. Eng. Mater. 2014, 16, 830–849. [Google Scholar] [CrossRef]
  16. Coble, R.L. Diffusion Models for Hot Pressing with Surface Energy and Pressure Effects as Driving Forces. J. Appl. Phys. 1970, 41, 4798–4807. [Google Scholar] [CrossRef]
  17. Krohn, D.A.; Urick, P.A.; Hasselman, D.P.H.; Langdon, T.G. Evidence for Coble creep in the relaxation of surface-compressive stresses in tempered polycrystalline aluminum oxide. J. Appl. Phys. 1974, 45, 3729–3731. [Google Scholar] [CrossRef]
  18. Cramer, C.L.; Aguirre, T.G.; Holland, T.B.; Ma, K. Prediction of continuous porosity gradients in ceramics using ZnO as a model material. J. Am. Ceram. Soc. 2018, 102, 587–594. [Google Scholar] [CrossRef]
  19. Pesce, A.; Hornés, A.; Núñez, M.; Morata, A.; Torrell, M.; Tarancón, A. 3D printing the next generation of enhanced solid oxide fuel and electrolysis cells. J. Mater. Chem. A 2020, 8, 16926–16932. [Google Scholar] [CrossRef]
  20. Ruiz-Morales, J.C.; Tarancón, A.; Canales-Vázquez, J.; Méndez-Ramos, J.; Hernández-Afonso, L.; Acosta-Mora, P.; Marín Rueda, J.R.; Fernández-González, R. Three dimensional printing of components and functional devices for energy and envi-ronmental applications. Energy Environ. Sci. 2017, 10, 846–859. [Google Scholar] [CrossRef] [Green Version]
  21. Sayan, Y.; Venkatesan, V.; Guk, E.; Wu, H.; Kim, J.-S. Single-step fabrication of an anode supported planar single-chamber solid oxide fuel cell. Int. J. Appl. Ceram. Technol. 2018, 15, 1375–1387. [Google Scholar] [CrossRef] [Green Version]
  22. Carazzone, J.R.; Bonar, M.D.; Baring, H.W.; Cantu, M.A.; Cordero, Z.C. In situ observations of cracking in con23 strained sintering. J. Am. Ceram. Soc. 2019, 102, 602–610. [Google Scholar]
  23. Li, H.; Liu, Y.; Liu, Y.; Zeng, Q.; Hu, K.; Lu, Z.; Liang, J. Effect of debinding temperature under an argon at-mosphere on the microstructure and properties of 3D-printed alumina ceramics. Mater. Charact. 2020, 168, 110548. [Google Scholar] [CrossRef]
  24. Ni, D.-W.; Esposito, V.; Schmidt, C.G.; Molla, T.T.; Andersen, K.; Kaiser, A.; Ramousse, S.; Pryds, N. Camber evolution and stress development of porous ceramic bi-layers during cofiring. J. Am. Ceram. Soc. 2013, 96, 972–978. [Google Scholar] [CrossRef]
  25. Kanters, J.; Eisele, U.; Rödel, J. Cosintering Simulation and Experimentation: Case Study of Nanocrystalline Zirconia. J. Am. Ceram. Soc. 2001, 84, 2757–2763. [Google Scholar] [CrossRef]
  26. Molla, T.; Frandsen, H.L.; Bjørk, R.; Ni, D.W.; Olevsky, E.; Pryds, N. Modeling kinetics of distortion in porous bi-layered structures. J. Eur. Ceram. Soc. 2013, 33, 1297–1305. [Google Scholar] [CrossRef] [Green Version]
  27. Olevsky, E.; Molla, T.T.; Frandsen, H.L.; Bjørk, R.; Esposito, V.; Ni, D.W.; Ilyina, A.; Pryds, N. Sintering of Multilayered Porous Structures: Part I-Constitutive Models. J. Am. Ceram. Soc. 2013, 96, 2657–2665. [Google Scholar] [CrossRef]
  28. Ni, D.W.; Olevsky, E.A.; Esposito, V.; Molla, T.T.; Foghmoes, S.P.; Bjork, R.; Frandsen, H.L.; Alexandrova, E.; Pryds, N. Sin-tering of multilayered porous structures: Part II—Experiments and model applications. J. Am. Ceram. Soc. 2013, 96, 2666–2673. [Google Scholar] [CrossRef]
  29. Molla, T.T.; Bjørk, R.; Olevsky, E.; Pryds, N.; Frandsen, H.L. Multi-scale modeling of shape distortions during sintering of bi-layers. Comput. Mater. Sci. 2014, 88, 28–36. [Google Scholar] [CrossRef]
  30. Shabana, Y.M.; Bruck, H.A.; Pines, M.L.; Kruft, J.G. Modeling the evolution of stress due to differential shrinkage in pow-der-processed functionally graded metal–ceramic composites during pressureless sintering. Int. J. Solids Struct. 2006, 43, 7852–7868. [Google Scholar] [CrossRef] [Green Version]
  31. Olevsky, E.A. Theory of sintering: From discrete to continuum. Mater. Sci. Eng. R: Rep. 1998, 23, 41–100. [Google Scholar] [CrossRef]
  32. Reddy, J.N. Theory and Analysis of Elastic Plates and Shells, 2nd ed.; CRC Press: Boca Raton, FL, USA, 2006. [Google Scholar]
Figure 1. A multilayered porous structure under uniaxial pressure, with the x–y plane as the geometrical mid-plane (only the x-axis is shown).
Figure 1. A multilayered porous structure under uniaxial pressure, with the x–y plane as the geometrical mid-plane (only the x-axis is shown).
Jcs 05 00053 g001
Figure 2. Porosity evolutions in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Figure 2. Porosity evolutions in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Jcs 05 00053 g002
Figure 3. Normalized thickness shrinkages in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Figure 3. Normalized thickness shrinkages in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Jcs 05 00053 g003
Figure 4. Normalized in-plane dimension evolution in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Figure 4. Normalized in-plane dimension evolution in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Jcs 05 00053 g004
Figure 5. Normalized stresses in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Figure 5. Normalized stresses in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.03 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Jcs 05 00053 g005
Figure 6. Porosity evolutions in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.1 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Figure 6. Porosity evolutions in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.1 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Jcs 05 00053 g006
Figure 7. Normalized thickness shrinkages in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.1 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Figure 7. Normalized thickness shrinkages in a symmetric, CGO_P/CGO_D/CGO_P tri-layer structure: (a) CGO_P layers, and (b) mid CGO_D layer (θ01 = 0.65, θ02 = 0.45, h01 = 0.4 mm, h02 = 0.1 mm, η02/η01 = 1, α2/α1 = 1, G2/G1 = 1).
Jcs 05 00053 g007
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Jin, Z.-H.; Cramer, C.L. A Lamination Model for Pressure-Assisted Sintering of Multilayered Porous Structures. J. Compos. Sci. 2021, 5, 53. https://doi.org/10.3390/jcs5020053

AMA Style

Jin Z-H, Cramer CL. A Lamination Model for Pressure-Assisted Sintering of Multilayered Porous Structures. Journal of Composites Science. 2021; 5(2):53. https://doi.org/10.3390/jcs5020053

Chicago/Turabian Style

Jin, Zhi-He, and Corson L. Cramer. 2021. "A Lamination Model for Pressure-Assisted Sintering of Multilayered Porous Structures" Journal of Composites Science 5, no. 2: 53. https://doi.org/10.3390/jcs5020053

Article Metrics

Back to TopTop