Article

SbI3·3S8: A Novel Promising Inorganic Adducts Crystal for Second Harmonic Generation

by
Tushar Kanti Das
1,*,
Marcin Jesionek
1,*,
Mirosława Kępińska
1,
Marian Nowak
1,
Michalina Kotyczka-Morańska
2,
Maciej Zubko
3,4,
Jarosław Młyńczak
5 and
Krzysztof Kopczyński
5
1
Institute of Physics—Center for Science and Education, Silesian University of Technology, Krasińskiego 8, 40-019 Katowice, Poland
2
Institute for Chemical Processing of Coal, Zamkowa 1, 41-803 Zabrze, Poland
3
Institute of Materials Engineering, Faculty of Science and Technology, University of Silesia, 75 Pułku Piechoty 1a, 41-500 Chorzów, Poland
4
Department of Physics, Faculty of Science, University of Hradec Králové, Rokitanského 62, 500 03 Hradec Králové, Czech Republic
5
Institute of Optoelectronics, Military University of Technology, Gen. Sylwestra Kaliskiego 2, 00-908 Warsaw, Poland
*
Authors to whom correspondence should be addressed.
Materials 2023, 16(3), 1105; https://doi.org/10.3390/ma16031105
Submission received: 2 January 2023 / Revised: 18 January 2023 / Accepted: 25 January 2023 / Published: 27 January 2023

Abstract

:
In the past twenty years, the basic investigation of innovative Non-Linear Optical (NLO) crystals has received significant attention, which has built the crucial heritage for the use of NLO materials. Fundamental research is essential given the scarcity of materials for NLO compounds, especially in the deep ultraviolet (DUV) and middle- and far-infrared (MFIR) regions. In the present work, we synthesized high-quality MFIR SbI3·3S8 NLO crystals having a length in the range of 1–5 mm through rapid facile liquid phase ultrasonic reaction followed by the assistance of instantaneous natural evaporation phenomenon of the solvent at room temperature. X-ray diffraction (XRD) results ratify the hexagonal R3m structure of SbI3·3S8 crystal, and energy-dispersive X-ray spectroscopy (EDX) demonstrates that the elemental composition of SbI3·3S8 crystal is similar to that of its theoretical composition. The direct and indirect forbidden energy gaps of SbI3·3S8 were measured from the optical transmittance spectra and they were shown to be 2.893 eV and 1.986 eV, respectively. The green sparkling signal has been observed from the crystal during the second harmonic generation (SHG) experiment. Therefore, as inorganic adducts are often explored as NLO crystals, this work on the MFIR SbI3·3S8 NLO crystal can bring about additional investigations on this hot topic in the near future.

1. Introduction

In recent years, the high demand for laser technology has drawn much more concentration on Non-Linear Optical (NLO) materials [1,2,3,4]. This application requires a large value of second-order non-linear (i.e creation of light at a second-harmonic frequency) vulnerability and an extended range of optical transparency [5,6,7]. The optical nonlinear compound with these characteristic features, which forms a noncentrosymmetric crystal structure in space, is of distinctive attraction [8,9,10]. To procure such an NLO crystal structure, the logical constructions of their elemental compositions are crucial. It is very well known that the coefficient of NLO is inversely proportional to the structural unit of the acentric crystallographic form [11,12]. Researchers are already trying to develop potential NLO crystals by combining two or more numbers of acentric structural units. The reason behind this combination of different structural units used to make NLO crystals is that different structural units exhibit various properties, and their combination provides such properties to NLO crystals [13,14,15].
Still, the developed deep ultraviolet (DUV) and middle- and far-infrared (MFIR) NLO crystals are inadequate to encounter the market requirements. There are many standard DUV NLO crystals available, such as KH2PO4, KBe2BO3F2, KTiOPO4, BPO4, β-BaB2O4, and KLa(PO3)4, which can satisfy basic necessity of the laser industry [6,16,17,18,19]. On the other hand, though the materials such as KBe2BO3F2, ZnGeP2, AgGaS2 (AGS), and AgGaSe2 (AGSe) have been used as DUV and MFIR NLO crystals, their ingrained obstructions harshly constrict their wide range of applications [20,21]. Among them, the most outstanding NLO crystal for MFIR is AGS and AGSe. However, they still have inherent defects, which make them a potential MFIR NLO material. Hence, it is essential to explore new promising MFIR NLO crystals with much more balance achieved.
The MFIR NLO crystals, which are prepared by chalcogenides, halides, and iodates, have a basic structural unit consisting of anions or anionic groups according to Chen’s anionic group hypothesis [22]. This type of crystal is basically formed either by conventional ionic or covalent bonds. The reason behind the fabrication of chalcogenides- and halides-based MFIR NLO crystals is that chalcogenides have a better NLO efficiency, but, in comparison with halides, they have small laser-induced damage thresholds (LIDT) [23]. Therefore, to overcome their deficiency, chalcogenides have been combined with halides in a specific ratio to obtain highly efficient MFIR NLO crystals [24]. Recently, a non-centrosymmetric adduct of MFIR NLO crystal known as antimony triiodide–octasulfur (SbI3·3S8) was explored, and it was found to display strong second-order non-linear properties [25], and the schematic non-centrosymmetric structure of the inorganic adduct SbI3·3S8 crystal is presented in Figure 1. SbI3·(S8)3 crystallizes in the trigonal noncentrosymmetric space group R3m. As presented in Figure 1, in one asymmetric structure unit, there are five S atoms, three I atoms, and one Sb atom. Two asymmetric structure units, trigonal-pyramidal SbI3 and chairlike S8, are bonded through van der Waals force interaction.
The nature of the essential MFIR NLO SbI3·3S8 crystals has been explored by several research groups. For example, Fernando et al. synthesized SbI3·3S8 crystal by the slow evaporation of the carbon disulphide from the constituent, but the quality of the crystals was not good [26]. Bjorvatten et al. also prepared the crystal through the same procedure and investigated its structure through the X-ray diffraction method only [27]. Currently, the crystals have also been fabricated by several other research groups through vapor phase reactions of antimony triiodide (SbI3) and sulfur (S), and the reactions were passed through a much more complicated and time-consuming process [25,28,29]. Based on the above background, we feel that it is essential to synthesize such MFIR NLO crystals through facile and rapid methods and explore their properties through practical SHG experiments.
In the present study, we demonstrate the synthesis of MFIR SbI3·3S8 crystals through a facile and rapid sonochemical process. We report, for the first time, the synthesis of MFIR SbI3·3S8 crystal from elemental antimony (Sb) sulfur (S), and iodine (I) by conducting sonochemical reaction in dichloromethane (CH2Cl2) as a solvent, and the natural phenomenon of rapid solvent evaporation helped in the formation of the crystal without the use of any other energy sources. The method is very simple and fast compared to others for producing the best quality SbI3·3S8 crystal with a high yield. The quality of the crystals was investigated by simple optical microscopy. The grown crystal was identified by X-ray diffraction studies and using the electron microscopic technique. The elemental compositions of the synthesized crystal and their distribution were diagnosed by an energy-dispersive X-ray spectroscopy (EDS) study. Direct and indirect forbidden energy gaps of the grown SbI3·3S8 crystals were measured by optical transmittance spectra. The second harmonic generation of light (SHG) in the grown crystals was also observed. We believe that the facile and rapid method of synthesis of MFIR NLO SbI3·3S8 crystal might be a potential candidate for the future of optoelectronic devices.

2. Materials and Methods

2.1. Materials

Antimony (Sb, 99.95%) was procured from Sigma–Aldrich. Sublimated sulfur (S), iodine (I), and dichloromethane (CH2Cl2) were bought from POCH S.A. (Gliwice, Poland). All the materials were used for experimental purposes without further purification. Ethanol and deionized water were engaged in the separation and purification process.

2.2. Synthesis of SbI3·3S8 Crystal

In a typical method, predetermined weights of antimony (Sb), sulfur (S), and iodine (I) were taken in 20 mL of dichloromethane (CH2Cl2) containing closed vessels and sonicated for 4 h in an ultrasonication bath. After sonication, the solution mixture was kept for 12 h for the settlement of solid particles. Later, the supernatant liquid was carefully poured into a Petri dish from the above portion of the mixture, and the Petri dish containing the supernatant liquid was kept in a nitrogen atmosphere for gradual evaporation of the solvent. As soon as we kept the Petri dish in the nitrogen atmosphere, the solvent instantly evaporated from the Petri dish with the formation of a yellow crystal, and the process of crystallization was completed within 2 h (at that same time evaporation of dichloromethane was completed). After the complete evaporation of the solvent, the grown crystals were collected from the Petri dish and kept in a closed chamber for further investigation and characterization purposes. The yield of the products was around 0.150 gm. The steps of SbI3·3S8 crystal formation starting from raw materials are schematically presented in Figure 2.

2.3. Characterization Techniques

Optical microscope imaging of the grown SbI3·3S8 crystals was performed with Stemi 2000-C Stereo Microscope (Zeiss, Germany) equipped with an Olympus DP25 camera (Olympus, Japan). Data acquisition from the microscope was performed using the Olympus Stream Basic 1.9 program. Powder X-ray diffraction (XRD) measurements of the grown SbI3·3S8 crystal were performed using a Panalytical Empyrean diffractometer (Malvern Instruments, Malvern, UK) with a Cu anode (with a wavelength of 1.54056 Å) working at an electric current of 30 mA and a voltage of 40 kV and equipped with an ultrafast solid-state hybrid detector (Malvern Instruments, Malvern, UK). The X-ray diffraction measurements were performed in an angular range of 2θ from 5° to 90° with a 0.02° step in Bragg–Brentano geometry (θ–θ scan technique), and the time count was 1000 s for each point at room temperature T ≈ 300 K. The morphology and elemental composition of the synthesized SbI3·3S8 crystal were examined by scanning electron microscopy (SEM) and energy-dispersive X-ray spectroscopy (EDX). These analyses were executed through the Phenom Pro X (Phenom World) microscope integrated with the EDX spectrometer. The peaks in the EDS spectrum were investigated by the ProSuite Element Identification (Phenom-World) computer program. The optical transmittance spectra of the SbI3·3S8 single crystals were measured at room temperature using the Flame spectrophotometer equipped with waveguide cables and the deuterium–halogen light source from Ocean Optics. Schematic diagram and a photo of the measuring station used to obtain the generation of the second harmonic of light are presented in Section 5. Second Harmonic Generation of Light in the SbI3·3S8. The source of 1064 nm radiation was an Nd:YAG/Cr:YAG microlaser pumped by a LIMO25-F100-LD808 laser diode with fiber optic output. The microlaser generated radiation pulses with a duration of 3 ns and energy of approx. 14 µJ. The repetition frequency varied linearly as a function of the pumping power. Radiation with a wavelength of 1064 nm was directed to the partitioning plate with a transmission of 94%. The reflected part of the radiation was recorded with an InGaAs ET-3000 photodiode to measure the temporal characteristics of the pulses. The output from the photodiode was observed on an Agilent Technologies MSO7104A oscilloscope. To eliminate the pumping radiation, the laser beam was directed to a dichroic mirror reflecting the radiation with a wavelength of 1064 nm.

3. Results

The optical microscopic (OM) images of the synthesized bright yellow branched SbI3·3S8 crystal as well, and single SbI3·3S8 crystals are presented in Figure 3a,b, respectively. The images clearly show that the length of the crystals varies in the range of 1–5 mm, while the diameter is in the range of 40–100 µm. When the single crystal is observed at a higher magnification by the optical microscope, a spherical drop is noticed at the end of the crystal, suggesting the termination of the crystallization process. Most likely, these droplets are formed by analogy to the mechanism of dew formation, e.g., on grass. Particles of crystal-forming substances settle on it. They form a thin layer that transforms into a droplet. For this to happen, the air temperature must drop below the dew point.
To reveal the crystallinity, purity, and crystallite size of the grown crystals, we performed an X-ray diffraction experiment, and the results are demonstrated in Figure 4. The sharp and distinct peaks indicate a well-defined crystallized structure of synthesized SbI3·3S8 crystal. The diffraction peaks are well-matched with the hexagonal R3m structure (PDF No. 71-2024), and the absence of other peaks indicates a high purity of the synthesized crystal [29]. The comparison between the crystal planes with diffraction angles (2θ) of the XRD experiment and the values obtained from standard 2θ of JCPDS (PDF No. 71-2024) of SbI3·3S8 crystal are summarized in Table 1. The table clearly shows that the theoretical and experimental values are similar, with minor deviations indicating a high purity of the crystals. To determine the interplanar spacing and crystallite size using Bragg’s law and the Debye–Scherrer equation, respectively, we use an exposed (110) crystal plane, and the measured value of the interplanar spacing and crystallite size are 1.22 nm and 282.17 nm, respectively.
To further study the morphology and internal composition of the SbI3·3S8 grown crystal, we examined the crystal using SEM, and the corresponding results are presented in Figure 5. Figure 5a shows groups of synthesized SbI3·3S8 crystals, and the images also show that the materials have slab-like structures with high purity and good crystallinity. The crystals are oriented in a particular direction. To achieve better morphology of the synthesized crystals, we examined the crystals under SEM after placing the crystal in a perpendicular direction to that of the silicon wafer, and the results are demonstrated in Figure 5b,c.
The figures show the well-aligned, uniform, and hexagonal morphology of SbI3·3S8 crystal without any impurity and a better outlook of the single crystal. To quantify the elemental composition of the as-grown SbI3·3S8 crystal, we performed an energy-dispersive X-ray spectroscopy (EDX) study during SEM analysis, and the results of this study are summarized in Figure 6. The EDX spectra show that the atomic ratio of S, I, and Sb in the synthesized SbI3·3S8 crystal is very close to 24:3:1, and the stoichiometric ratio of the elements in the crystal have good similarity with the theoretical composition of SbI3·3S8 crystal. The distribution of elements throughout the crystal was examined using elemental mapping, and the corresponding outcomes are demonstrated in Figure 7. The elemental mapping reports a uniform distribution of S, I, and Sb in the whole crystal. The results of the SEM study confirm the successful synthesis of SbI3·3S8 crystal.
Figure 8 presents the absorbance spectra of one of the SbI3·3S8 single crystals calculated from optical transmittance. Applying the method of simultaneous fitting of many absorption mechanisms to the spectral dependence of absorbance [25], these data were used to determine the optical energy gap of the SbI3·3S8 single crystal. The red curve from Figure 8 presents the best-fitted theoretical dependence of the investigated SbI3·3S8 single crystal appropriate for the sum of indirect forbidden absorption without excitons or phonon statistics (α1), direct forbidden absorption without excitons (α2), Urbach absorption (α3), and constant absorption term (α4) [30]:
α 1 = A 60 h ν E g I f 3   f o r   h ν > E g I f
  α 2 = A 3 h ν ( h ν E g D f ) 3 / 2   f o r   h ν > E g D f
  α 3 = A U exp h ν E U   = A exp B h ν C k B T  
α 4 = A 0
where EgIf represents the indirect forbidden energy gap; EgDf is the direct forbidden energy gap; EU is the Urbach energy; and A60, A3, and AU are constant parameters. The constant absorption term A0 is an attenuation coefficient that is considered the sum of the scattering and absorption independent of photon energy (hν) near the absorption edge. The values of the fitted parameters are: EgDf = 2.893 eV, EgIf = 1.986 eV, EU = 38.8 meV, A3 = 73.4 eV−1/2, A60 = 1.665 eV−3, AU = 1.609 × 10−3, and A0 = 1.045.

4. Plausible Mechanism of Formation of SbI3·3S8 Crystal in CH2Cl2

The possible mechanism of SbI3·3S8 crystal formation from elemental Sb, S, and I in dichloromethane as a solvent medium under ultrasonic irradiation can be described as follows:
(i)
First, due to the high reactivity tendency of iodine (I) and antimony (Sb), they easily react with each other in dichloromethane (CH2Cl2) to form antimony tri-iodide (SbI3).
2Sb + 3I2 Materials 16 01105 i0012SbI3
(ii)
At the same time, during ultrasonication, CH2Cl2 will break down into various reactive radical species [31]. The steps of radical formation are given below:
CH2Cl2 Materials 16 01105 i002H· + ·CHCl2
H· + CH2Cl2 Materials 16 01105 i002H2 ↑ + ·CHCl2
(iii)
In the next step, the highly reactive radicals react with iodine molecules of SbI3 molecules through the formation of an adduct compound. The intermediate compounds are very unstable and tend to react further.
SbI3+3·CHCl2 Materials 16 01105 i002SbI3·3CHCl2
(iv)
On the other side, when ultrasonic waves passed through a liquid medium, they stretched and compressed the molecules in which they were transmitted. During the stretching period, negative pressure is created on the liquid medium and at a specific pressure; they produced microbubbles when the pressure surpassed the intermolecular binding forces of liquid molecules. In the next cycles of stretching and compression, these microbubbles grew continuously and decomposed near the surface of the elemental sulfur. During the decomposition of these bubbles, they generated high temperature and pressure, which is responsible for the cleavage of elemental sulfur into small S8 molecules [32].
Elemental sulfur Materials 16 01105 i001nS8
(v)
These highly reactive small S8 molecules can gradually diffuse near the unstable SbI3·3CHCl2 adduct compound, and they reacted through a substitution reaction to form SbI3·3S8 nuclei.
3S8 + SbI3·3CHCl2 Materials 16 01105 i001SbI3·3S8
(vi)
The formed nuclei are unstable in the solvent medium, and they always have a propensity to grow as SbI3·3S8 crystals along a specific axis by sharing lone pair electrons of Sb molecules. Room temperature evaporation of the solvent (CH2Cl2), as well as the attraction of lone pairs, helps in the formation of a one-dimensional crystal structure by pushing the nuclei to each other. Finally, we obtained the grown crystal, which is one-dimensional and highly anisotropic in nature [27,33].
The steps of the plausible formation mechanism of SbI3·3S8 crystals are also schematically presented in Figure 9.

5. Second Harmonic Generation of Light in the SbI3·3S8

A radiation level of 1064 nm was focused on the test material using a lens with a focal length of 35 mm. The examined crushed pieces of SbI3·3S8 crystals were placed in a glass container (with a transmitting radiation of 1064 nm and 532 nm) on a micrometric table, enabling movement on three axes. Behind the tested sample, there were band-stop and band-rejection Notch filters (NF1064-44—Ø25 mm Notch Filter, CWL = 1064 nm, FWHM = 44 nm, ThorLabs) that cut off 1064 nm radiation while maintaining high transmission at 532 nm radiation. The radiation of 532 nm was carried by a fiber with a core diameter of 230 µm to a computer-controlled Avantes AvaSpec-3648 spectrometer. The schematic diagram with pathways of lights and a digital image of the experimental set up are presented in Figure 10a,b. The photo in Figure 10c shows a green glowing signal SbI3·3S8 crystal. The generation spectrum is shown in Figure 10d. The spectrum shows that the intensity of the peak is much higher than previously published results [20,28], which accounts for the high purity of the synthesized SbI3·3S8 crystals.

6. Conclusions

In summary, an inorganic adduct of MFIR SbI3·3S8 crystals was synthesized by a facile liquid phase reaction through the consecutive combined action of the ultrasonic irradiation and evaporation method for the first time from the individual elements (Sb, I, and S). The formation of SbI3·3S8 crystals was confirmed by various well-known characterized techniques, and based on this, a probable mechanism of the crystals is represented. The study of the NLO properties suggests SbI3·3S8 crystals exhibit a second-harmonic generation response, which is presented as a potential candidate for NLO crystals in the MFIR region. Virtually, this work broadly scrutinized an MFIR NLO crystal, and their exceedingly encouraging NLO properties and the need for consideration of all-inorganic adduct-type NLO properties project a critical inquiry about subgroups for investigation of novel NLO crystals. It is anticipated that this work can inspire more analysis of seldom-touched inorganic adducts. Moreover, its basic chemical composition, simple synthesis, and high productivity make it one of the foremost promising MFIR NLO crystals for futuristic optoelectronic devices. The results presented, and in particular the new fast and cheap method of SbI3·3S8 production, may constitute the basis for more detailed research on the SHG phenomenon observed in this material.

Author Contributions

T.K.D.: Conceptualization, Methodology, Formal analysis, Investigation, Writing—Original Draft, Supervision. M.J.: Formal analysis, Investigation, Writing—Original Draft, Supervision, Funding acquisition. M.K.: Investigation, Writing—Review and Editing. M.N.: Supervision, Visualization. M.K.-M.: Investigation. M.Z.: Investigation. J.M.: Investigation. K.K.: Investigation. All authors have read and agreed to the published version of the manuscript.

Funding

This research is partially funded by the Silesian University of Technology (Gliwice, Poland) and the Rector’s Pro-Quality Grant Program 14/010/RGJ22/0009.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All data presented in this study are included in the published article.

Acknowledgments

T.K. Das and M. Jesionek thank the Silesian University of Technology for providing the facility and financial support to carry out my research at the Division of Solid State Physics, Institute of Physics—Center for Science and Education. This research is also partially funded by the Silesian University of Technology (Gliwice, Poland) and the Rector’s Pro-Quality Grant Program 14/010/RGJ22/0009.

Conflicts of Interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

References

  1. Kang, L.; Liang, F.; Jiang, X.; Lin, Z.; Chen, C. First-principles design and simulations promote the development of nonlinear optical crystals. Acc. Chem. Res. 2019, 53, 209–217. [Google Scholar] [CrossRef]
  2. Kang, L.; Lin, Z. Deep-ultraviolet nonlinear optical crystals: Concept development and materials discovery. Light Sci. Appl. 2022, 11, 201. [Google Scholar] [CrossRef]
  3. Mutailipu, M.; Poeppelmeier, K.R.; Pan, S. Borates: A rich source for optical materials. Chem. Rev. 2020, 121, 1130–1202. [Google Scholar] [CrossRef] [PubMed]
  4. Xu, B.; Li, Z.; Wang, K.; Zhang, J.; Liang, L.; Li, L.; Ren, Y.; Liu, Y.; Liu, M.; Xue, D. Growth and Optical Properties of the Whole System of Li (Mn1−x, Nix) PO4 (0 ≤ x ≤ 0.5) Single Crystals. Materials 2021, 14, 7233. [Google Scholar] [CrossRef]
  5. Shen, Y.; Zhao, S.; Luo, J. The role of cations in second-order nonlinear optical materials based on π-conjugated [BO3]3− groups. Coord. Chem. Rev. 2018, 366, 1–28. [Google Scholar] [CrossRef]
  6. Guo, S.-P.; Chi, Y.; Guo, G.-C. Recent achievements on middle and far-infrared second-order nonlinear optical materials. Coord. Chem. Rev. 2017, 335, 44–57. [Google Scholar] [CrossRef]
  7. Zhao, J.; Wu, J.; Chen, X.; Zeng, R. Effect of Temperature on Ultrasonic Nonlinear Parameters of Carbonated Concrete. Materials 2022, 15, 8797. [Google Scholar] [CrossRef]
  8. Samoc, A.; Samoc, M.; Luther-Davies, B.; Kelly, J.; Krausz, E.; Willis, A. New second-order nonlinear octupolar materials. Mol. Cryst. Liq. Cryst. 2004, 415, 179–195. [Google Scholar] [CrossRef]
  9. Lin, H.; Zheng, Y.J.; Hu, X.N.; Chen, H.; Yu, J.S.; Wu, L.M. Non-centrosymmetric Selenides AZn4In5Se12 (A = Rb, Cs): Synthesis, Characterization and Nonlinear Optical Properties. Chem. Asia. J. 2017, 12, 453–458. [Google Scholar] [CrossRef]
  10. Liu, K.; Kang, Y.; Tao, H.; Zhang, X.; Xu, Y. Effect of Se on Structure and Electrical Properties of Ge-As-Te Glass. Materials 2022, 15, 1797. [Google Scholar] [CrossRef] [PubMed]
  11. Chung, I.; Kanatzidis, M.G. Metal chalcogenides: A rich source of nonlinear optical materials. Chem. Mater. 2014, 26, 849–869. [Google Scholar] [CrossRef]
  12. Yu, H.; Koocher, N.Z.; Rondinelli, J.M.; Halasyamani, P.S. Pb2BO3I: A Borate Iodide with the Largest Second-Harmonic Generation (SHG) Response in the KBe2BO3F2 (KBBF) Family of Nonlinear Optical (NLO) Materials. Angew. Chem. Int. Ed. 2018, 57, 6100–6103. [Google Scholar] [CrossRef] [PubMed]
  13. Pan, Y.; Guo, S.-P.; Liu, B.-W.; Xue, H.-G.; Guo, G.-C. Second-order nonlinear optical crystals with mixed anions. Coord. Chem. Rev. 2018, 374, 464–496. [Google Scholar] [CrossRef]
  14. Sun, Z.-D.; Chi, Y.; Xue, H.-G.; Guo, S.-P. A Series of Pentanary Inorganic Supramolecular Sulfides (A3X) [MB12(MS4)3] (A = K, Cs; X = Cl, Br, I; M = Ga, In, Gd) Featuring B12S12 Clusters. Inorg. Chem. Front. 2017, 4, 1841–1847. [Google Scholar] [CrossRef]
  15. Scherbak, S.A.; Kaasik, V.P.; Zhurikhina, V.V.; Lipovskii, A.A. Poling of Glasses Using Resistive Barrier Discharge Plasma. Materials 2022, 15, 8620. [Google Scholar] [CrossRef] [PubMed]
  16. Sekar, A.; Muthurakku, U.R.; Sivaperuman, K. An Overview on Recent Trends in Deep-Ultraviolet (DUV) and Ultraviolet (UV) Nonlinear Optical Crystals. ChemistrySelect 2021, 6, 10688–10716. [Google Scholar] [CrossRef]
  17. Mutailipu, M.; Yang, Z.; Pan, S. Toward the enhancement of critical performance for deep-ultraviolet frequency-doubling crystals utilizing covalent tetrahedra. Acc. Mater. Res. 2021, 2, 282–291. [Google Scholar] [CrossRef]
  18. Janarthanan, S.; Samuel, R.S.; Selvakumar, S.; Rajan, Y.; Jayaraman, D.; Pandi, S. Growth and characterization of organic NLO crystal: β-naphthol. J. Mater. Sci. Technol. 2011, 27, 271–274. [Google Scholar] [CrossRef]
  19. Almuqrin, A.H.; Gangareddy, J.; Hivrekar, M.M.; Pramod, A.; Sayyed, M.; Keshavamurthy, K.; Fatima, N.; Jadhav, K. Nonlinear Optical Limiting and Radiation Shielding Characteristics of Sm2O3 Doped Cadmium Sodium Lithium Borate Glasses. Materials 2022, 15, 2330. [Google Scholar] [CrossRef]
  20. Lu, Z.-T.; Sun, Z.-D.; Chi, Y.; Xue, H.-G.; Guo, S.-P. Balanced second-order nonlinear optical properties of adducts CHI3·(S8)3 and AsI3·(S8)3: A systematic survey. Inorg. Chem. 2019, 58, 4619–4625. [Google Scholar] [CrossRef]
  21. Shui, Q.R.; Fu, R.B.; Zhou, Z.Q.; Ma, Z.J.; Tang, H.X.; Wu, X.T. A Lead Mixed Halide with Three Different Coordinated Anions and Strong Second-Harmonic Generation Response. Chem. Euro. J. 2022, 28, e202103687. [Google Scholar] [CrossRef]
  22. Chen, C.; Wu, Y.; Li, R. The anionic group theory of the non-linear optical effect and its applications in the development of new high-quality NLO crystals in the borate series. Int. Rev. Phys. Chem. 1989, 8, 65–91. [Google Scholar] [CrossRef]
  23. Yan, M.; Xue, H.-G.; Guo, S.-P. Recent achievements in lone-pair cation-based infrared second-order nonlinear optical materials. Cryst. Growth Des. 2020, 21, 698–720. [Google Scholar] [CrossRef]
  24. Xiao, J.-R.; Yang, S.-H.; Feng, F.; Xue, H.-G.; Guo, S.-P. A review of the structural chemistry and physical properties of metal chalcogenide halides. Coord. Chem. Rev. 2017, 347, 23–47. [Google Scholar] [CrossRef]
  25. Nowak, M.; Kotyczka-Morańska, M.; Szperlich, P.; Jesionek, M.; Kępińska, M.; Stróż, D.; Kusz, J.; Szala, J.; Moskal, G.; Rzychoń, T.; et al. Using of sonochemically prepared components for vapor phase growing of SbI3·3S8. Ultrason. Sonochemistry 2010, 17, 892–901. [Google Scholar] [CrossRef] [PubMed]
  26. Fernando, W. Single crystal Raman spectra of SbI3·3S8; CHI3·3S8 and AsI3·3S8. J. Inorg. Nucl. Chem. 1981, 43, 1141–1145. [Google Scholar] [CrossRef]
  27. Bjorvatten, T.; Hassel, O.; Lindheim, A. Crystal structure of addition compound SBI3/3S8. Acta Chem. Scand. 1963, 17, 689–702. [Google Scholar] [CrossRef]
  28. Guo, S.-P.; Sun, Z.-D.; Chi, Y.; Xue, H.-G. Adduct-type IR nonlinear-optical crystal SbI3·(S8)3 with a large second-harmonic generation and a high laser-induced damage threshold. Inorg. Chem. 2018, 57, 11282–11288. [Google Scholar] [CrossRef]
  29. Feng, X.; Sun, Z.; Pei, K.; Han, W.; Wang, F.; Luo, P.; Su, J.; Zuo, N.; Liu, G.; Li, H. 2D inorganic bimolecular crystals with strong in-plane anisotropy for second-order nonlinear optics. Adv. Mater. 2020, 32, 2003146. [Google Scholar] [CrossRef]
  30. Kotyczka-Morańska, M.; Nowak, M.; Kępińska, M.; Szperlich, P.; Szala, J. Własności optyczne monokryształów SbI3·3S8 otrzymanych z fazy gazowej. Inż. Mater. 2008, 29, 127–130. [Google Scholar]
  31. Lim, M.; Son, Y.; Khim, J. Frequency effects on the sonochemical degradation of chlorinated compounds. Ultrason. Sonochem. 2011, 18, 460–465. [Google Scholar] [CrossRef] [PubMed]
  32. Warren, B.; Burwell, J. The structure of rhombic sulphur. J. Chem. Phys. 1935, 3, 6–8. [Google Scholar] [CrossRef]
  33. Gedanken, A. Using sonochemistry for the fabrication of nanomaterials. Ultrason. Sonochem. 2004, 11, 47–55. [Google Scholar] [CrossRef] [PubMed]
Figure 1. Schematic diagram of SbI3·3S8 crystal structure.
Figure 1. Schematic diagram of SbI3·3S8 crystal structure.
Materials 16 01105 g001
Figure 2. Digital images of each step of the synthesis of SbI3·3S8 crystal.
Figure 2. Digital images of each step of the synthesis of SbI3·3S8 crystal.
Materials 16 01105 g002
Figure 3. Optical microscopic images of grown (a) branches and (b) single SbI3·3S8 crystals.
Figure 3. Optical microscopic images of grown (a) branches and (b) single SbI3·3S8 crystals.
Materials 16 01105 g003
Figure 4. X-ray diffraction (XRD) pattern of prepared SbI3·3S8 crystal (The peaks are marked with crystal planes and below provide the JCPDS (PDF No. 71-2024) of SbI3·3S8 crystal).
Figure 4. X-ray diffraction (XRD) pattern of prepared SbI3·3S8 crystal (The peaks are marked with crystal planes and below provide the JCPDS (PDF No. 71-2024) of SbI3·3S8 crystal).
Materials 16 01105 g004
Figure 5. (a) SEM image of the branch of SbI3·3S8 crystal. (b,c) SEM images of a single SbI3·3S8 crystal after rotating the silicon wafer at a specific angle.
Figure 5. (a) SEM image of the branch of SbI3·3S8 crystal. (b,c) SEM images of a single SbI3·3S8 crystal after rotating the silicon wafer at a specific angle.
Materials 16 01105 g005
Figure 6. (a) SEM image of SbI3·3S8 crystal and (b) energy-dispersive X-ray spectroscopy (EDS) of SbI3·3S8 crystal (inset of the EDS spectrum demonstrates the atomic concentration and weight concentration of each element present in the crystal).
Figure 6. (a) SEM image of SbI3·3S8 crystal and (b) energy-dispersive X-ray spectroscopy (EDS) of SbI3·3S8 crystal (inset of the EDS spectrum demonstrates the atomic concentration and weight concentration of each element present in the crystal).
Materials 16 01105 g006
Figure 7. (a) SEM image and (b) EDS mapping and elemental analysis including (b1) sulfur (S), (b2) iodine (I), (b3) antimony (Sb), and (b4) EDS spectrum (inset shows the atomic concentration and weight concentration of each element present in the crystal) of the SbI3·3S8 crystal.
Figure 7. (a) SEM image and (b) EDS mapping and elemental analysis including (b1) sulfur (S), (b2) iodine (I), (b3) antimony (Sb), and (b4) EDS spectrum (inset shows the atomic concentration and weight concentration of each element present in the crystal) of the SbI3·3S8 crystal.
Materials 16 01105 g007
Figure 8. Absorbance spectrum of SbI3·3S8 single crystal measured at room temperature. The solid curve represents the least square fitted theoretical dependences for the sum of constant absorption term, direct and indirect forbidden absorptions, and Urbach ruled absorption (description and values of the fitted parameters are given in the text).
Figure 8. Absorbance spectrum of SbI3·3S8 single crystal measured at room temperature. The solid curve represents the least square fitted theoretical dependences for the sum of constant absorption term, direct and indirect forbidden absorptions, and Urbach ruled absorption (description and values of the fitted parameters are given in the text).
Materials 16 01105 g008
Figure 9. Schematic diagram of the crystal the mechanism of grown SbI3·3S8 crystal starting from raw materials (antimony (Sb), iodine (I), and sulfur (S)) in dichloromethane (CH2Cl2) as a solvent medium.
Figure 9. Schematic diagram of the crystal the mechanism of grown SbI3·3S8 crystal starting from raw materials (antimony (Sb), iodine (I), and sulfur (S)) in dichloromethane (CH2Cl2) as a solvent medium.
Materials 16 01105 g009
Figure 10. (a) Schematic diagram of the experimental set-up of SHG. (b) Digital image of the test stand for SHG generation in SbI3·3S8 crystals, (c) a shining piece of the crystal SbI3·3S8 during the generation of the second harmonic of light, and (d) spectral characteristics of the second harmonic of light generation for the repetition frequency of 0.85 kHz.
Figure 10. (a) Schematic diagram of the experimental set-up of SHG. (b) Digital image of the test stand for SHG generation in SbI3·3S8 crystals, (c) a shining piece of the crystal SbI3·3S8 during the generation of the second harmonic of light, and (d) spectral characteristics of the second harmonic of light generation for the repetition frequency of 0.85 kHz.
Materials 16 01105 g010
Table 1. Comparison of a diffraction angle (2Ɵ) from the results obtained from the XRD experiment with standard values for the SbI3·3S8 crystal.
Table 1. Comparison of a diffraction angle (2Ɵ) from the results obtained from the XRD experiment with standard values for the SbI3·3S8 crystal.
SL. No.Crystal PlanesObserved 2Ɵ from XRD Experiment (Degree)Standard 2Ɵ from JCPDS (PDF No. 71-2024) (Degree)
hkl
1.1107.2827.118
2.30012.35012.345
3.22014.34414.264
4.14018.90918.907
5.02121.89021.690
6.06024.78224.836
7.52025.77925.868
8.05128.96228.962
9.24129.94729.826
10.51130.64430.702
11.17031.34031.399
12.43132.65032.390
13.16134.02734.004
14.55036.12136.166
15.90037.61037.637
16.28038.30738.354
17.47040.28940.441
18.66043.67143.761
19.93045.46645.620
20.15247.43547.292
21.61249.58649.652
22.53250.83550.801
23.77051.52351.513
24.111153.32153.289
25.68155.80855.997
26.112157.69857.580
27.56258.78658.392
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Das, T.K.; Jesionek, M.; Kępińska, M.; Nowak, M.; Kotyczka-Morańska, M.; Zubko, M.; Młyńczak, J.; Kopczyński, K. SbI3·3S8: A Novel Promising Inorganic Adducts Crystal for Second Harmonic Generation. Materials 2023, 16, 1105. https://doi.org/10.3390/ma16031105

AMA Style

Das TK, Jesionek M, Kępińska M, Nowak M, Kotyczka-Morańska M, Zubko M, Młyńczak J, Kopczyński K. SbI3·3S8: A Novel Promising Inorganic Adducts Crystal for Second Harmonic Generation. Materials. 2023; 16(3):1105. https://doi.org/10.3390/ma16031105

Chicago/Turabian Style

Das, Tushar Kanti, Marcin Jesionek, Mirosława Kępińska, Marian Nowak, Michalina Kotyczka-Morańska, Maciej Zubko, Jarosław Młyńczak, and Krzysztof Kopczyński. 2023. "SbI3·3S8: A Novel Promising Inorganic Adducts Crystal for Second Harmonic Generation" Materials 16, no. 3: 1105. https://doi.org/10.3390/ma16031105

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop