Next Article in Journal
Effects of Curing Temperature on Expansion of Concrete Due to ASR
Next Article in Special Issue
Principles and Methods for Improving the Thermoelectric Performance of SiC: A Potential High-Temperature Thermoelectric Material
Previous Article in Journal
Bonding Efficiency between Artificial Teeth and Denture Base in CAD/CAM and Conventional Complete Removable Dentures
Previous Article in Special Issue
Oxide Scale Microstructure and Scale Growth Kinetics of the Hot-Pressed SiBCN-Ti Ceramics Oxidized at 1500 °C
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effects of Alumina Bubble Addition on the Properties of Corundum–Spinel Castables Containing Cr2O3

1
School of Materials Science and Engineering, Henan Key Laboratory of High Temperature Functional Ceramics, Zhengzhou University, Zhengzhou 450001, China
2
Administration for Market Regulation of Xihua County, Xihua, Zhoukou 466600, China
*
Authors to whom correspondence should be addressed.
Materials 2024, 17(13), 3139; https://doi.org/10.3390/ma17133139
Submission received: 7 May 2024 / Revised: 9 June 2024 / Accepted: 24 June 2024 / Published: 27 June 2024

Abstract

:
Purging plugs made of corundum–spinel castables containing Cr2O3 have been widely utilized in secondary refining process. However, their poor thermal shock resistance has greatly limited the improvement of their service life. Aiming to enhance their properties, we introduced alumina bubbles (ABs) to corundum–spinel castables, and the effects of the AB addition on the properties of the castables are studied in this manuscript. The results indicate that the apparent porosity, permanent linear change, cold strength, and hot strength all increased with an increasing AB amount. The thermal shock resistance of the samples with the AB addition was improved; the residual strength and residual strength ratio of the sample with 4 wt% ABs was the best. The effects of ABs on the tabular alumina aggregate distribution and relationship between the cold strength of the samples and the AB content was evaluated via the box dimension method. With the increments of AB content, the box dimension value of the tabular alumina within the samples significantly decreased, indicating that the tabular alumina aggregate distribution was related to the amount of ABs. In addition, the relationship between the box dimension and the strength was also established.

1. Introduction

Purging plugs play a crucial role in secondary refining processes to produce high-quality steel; their functions include facilitating reactions, discharging harmful gases, separating impurities from molten steel, and stirring the molten steel in steel ladles via flowing argon gas [1,2]. Unfortunately, the service life of purging plugs is dramatically shorter in comparison to that of steel ladle linings because of their severe working environment, including thermal stress derived from a larger temperature gradient, corrosion by slag and molten steel, and severe erosion wear by the oxygen cleaning process [3,4,5]. To meet the strict requirements, corundum–spinel castables containing Cr2O3 have been widely used to fabricate purging plugs due to their impressive slag resistance and excellent hot strength [6], but their poor thermal shock resistance (TSR) results in thermal spalling and fracture, thereby reducing their service life [7]. To respond to these issues, some attempts have been made to improve the TSR of corundum–spinel castables, such as adding zirconia, zirconia–alumina, alumina nanopowders, etc. [8,9,10,11]; however, the TSR of the castables needs to be further enhanced.
Refractory aggregates make up a larger proportion in castables, generally about 70 wt%, which greatly influences their properties. Recently, some works have been conducted to enhance their properties by changing the type and amount of corundum–spinel aggregates in castables. For instance, Tang et al. [12] added porous multi-component CaO-MgO-Al2O3 aggregates into castables and found that the bonding of interfaces between the aggregates and the matrix was strengthened and that small pores in aggregates can remit thermal stress, resulting in an incensement of the TSR of the specimens. Chen et al. [13] found that the thermal conductivity of corundum–spinel castables was reduced and the TSR was improved by adding porous corundum spheres with a microporous shell and macroporous core. Liu et al. [14] revealed that corundum–spinel castables containing as-formed bonite (CA6) aggregates resulted in good TSR, which was due to the released thermal stress and deviated cracks by CA6 flakes and their micropores. Liu et al. [15] found that alumina–spinel castables with resin-coated tabular alumina aggregates possessed an improved TSR, which, due to the micro-space formed along the boundary of the aggregates and matrices, can alleviate thermal stress, prolonging the crack propagation path and decelerating the crack propagation rate. Unfortunately, these castables still face some challenges, including a high cost and complex procedures. Hence, selecting a commercial aggregate to cope with industrial requirements should be more feasible.
Alumina bubbles (ABs) have been commonly used to fabricate porous corundum bricks and lightweight thermal insulation refractories due to their excellent performance of lower bulk density, lower apparent porosity, and higher closed porosity [16,17]. For example, Li et al. [18] attempted to introduce ABs into mullite castables and found that the residual strength ratio of the castables could be improved from 63.2% to 88.6%. Herein, ABs were added into corundum–spinel castables, and the effect of the AB content and heat treatment temperature on the physical properties and high-temperature properties of the corundum–spinel castables are studied in this manuscript. The results demonstrate that decrease in the thermal conductivity and the improvement of the TSR of corundum–spinel castables can be obtained by adding ABs, due to the ABs possessing a lower bulk density, a spherical shape, and a hollow structure.

2. Experimental

2.1. Material Preparation and Characterization

Tabular alumina aggregates (6–3 mm, 3–1 mm, 1–0.5 mm, and 0.5–0 mm, Almatis, Qingdao, China), alumina bubbles (1–0.5 mm, bulk density: 0.95 g/cm3, Henan Sicheng Yanmo Co., Zhengzhou, China), fused spinel powder (MgO: 25%, <0.074 mm, Luoyang Lier Co., Luoyang, China), white corundum powder (Al2O3: 99.0%, <0.088 mm, Kaifeng Tenai Co., Kaifeng, China), ultrafine alumina (Al2O3 > 99.5%, d50 = 1.2 µm, Henan Tianma Co., Zhengzhou, China), chromia powder (Cr2O3 > 98%, <20 μm, Luoyang Zhengjie Co., Luoyang, China), and calcium aluminate cement (Secar 71, Imerys, Tianjin, China) were used as raw materials.
The mass ratio of the aggregates (25% 6–3 mm, 25% 3–1 mm, 10% 1–0.5 mm, and 10% 0.5–0 mm) and the matrix was 70:30 in the castables. The 1–0.5 mm tabular alumina aggregates were replaced by ABs, at amounts of 0 wt% (0 Vol%), 2 wt% (7 Vol%), 4 wt% (13.3 Vol%) and 6 wt% (19.0 Vol%). The specimens were coded as AB0, AB2, AB4, and AB6, respectively. Firstly, the aggregates and matrices were uniformly mixed and blended with water, and then the mixtures were cast into 25 mm × 25 mm × 150 mm bars. Subsequently, they were demolded after aging in ambient air for 24 h, and dried at 110 °C for 24 h. Finally, they were calcined at 1100 °C, 1400 °C, and 1600 °C for 3 h, respectively.
The physical properties of the castables, including the apparent porosity (AP), bulk density (BD), permanent linear change (PLC), cold modulus of rupture (CMOR), and cold crushing strength (CCS) were carried out. The AP and BD were identified according to GB/T2997-2015. The PLC was evaluated according to GB/T5988-2022. The CMOR and CCS were measured at room temperature according to GB/T3001-2017 and GB/T5072-2008, respectively. The hot modulus of rupture (HMOR) was identified according to GB/T3002-2017 at 1400 °C for 0.5 h via the 3-point bending method. In addition, the TSR of the castables after heating at 1600 °C was evaluated at 1100 °C for 0.5 h using the water quenching method, and the residual CMOR (CMORst) and retained strength ratios (RSR) were measured.
The microstructures of the fracture specimens and the polished cross-sections (embedded in the resin) of the samples and ABs were characterized by a scanning electron microscope (SEM, TESCAN MIRA LMS, Brno, Czech Republic) equipped with an energy-dispersive spectrometer (EDS, Oxford Xplore, Oxford, UK). The phase composition of the specimens was examined by X-ray diffraction (XRD, Philips X′Pert, Almelo, The Netherlands) with Cu Kα radiation (λ = 1.5406 Å) at 40 kV, 40 mA, and a scan range of 10°−80° at 10°/min.

2.2. Fractal Method

Fractal theory, as a quantitative approach, directly reveals the inherent laws within complex and irregular systems, such as irregular and coarse geometric shapes in nature [19,20]. Hence, fractal theory has diverse applications in numerous disciplines, notably in the realm of material science. Its utility spans the characterization of pores in porous materials [21,22,23], cracks [24,25], and other morphology analyses. The box-counting dimension method is a prevalent technique for calculating the box dimension (Db) of structures, facilitating the computation of dimensions for complex structures or shapes.
Let F be any bounded non-empty subset of Rn, where Nδ(F) represents the minimum number of boxes that are required to encompass F with the box edge length δ (δ > 0). The relationship between Nδ(F) and δ can be defined as Equation (1) [26,27]:
N δ ( F ) δ D b
where Db is the box dimension. The opposite number of the limit of lnNδ(F)/lnδ as δ approaches 0 is Db. By selecting the δ of different scales, the continuous point graph of (lnNδ(F), lnδ) can be obtained. At a small scale, lnNδ(F) and lnδ are linearly dependent, and Equation (1) can be equivalent to Equation (2):
D b d ln N δ F d ln δ
Therefore, the negative of the slope of the line obtained from linear regression on the scatter plot is denoted as Db.
In this work, the cross-sections of the castables fired at 1600 °C were selected and recorded by a digital camera. Image processing software was utilized to capture high-resolution images of the samples, and the tabular alumina aggregates and matrices were distinguished by highlighting them in white and black, respectively.

3. Results and Discussion

3.1. Characterization of Alumina Bubbles

Figure 1 shows the microstructures of the ABs. As shown in Figure 1a–c, the AB particles were hollow and spherical, the shell thickness of the ABs was about 83.5 µm, and small pores were observed on their surface. The internal morphologies of the ABs are shown in Figure 1d; it can be observed that the shells of the ABs were dense and shaped by stacking cubic alumina crystals. Their phase composition was corundum (ICDD No. 00-011-0661) (Figure 1e). As shown in Figure 1f, some ABs floated on the surface of water, whereas others sank to the bottom, suggesting that a certain number of the ABs were broken.

3.2. Physical Properties of the Castables

Figure 2 presents the physical properties of the samples treated at different temperatures. As shown in Figure 2a,b, as the ABs increased, the AP values of the castables after heat-treating at 110 °C, 1100 °C, 1400 °C, and 1600 °C increased from 11.5% to 12.7%, from 13.3% to 18.3%, from 15.3% to 19.5%, and from 13.6% to 18.8%, respectively, which may have been due to the presence of surface pores on the ABs. Additionally, the hollow structure of the ABs was partially destroyed during the mixing process, thereby increasing the apparent porosity. In contrast, the BD exhibited a corresponding downward trend, decreasing from 3.28 g/cm3 to 3.10 g/cm3, from 3.26 g/cm3 to 3.09 g/cm3, from 3.22 g/cm3 to 3.07 g/cm3, and from 3.28 g/cm3 to 3.09 g/cm3, which may have been because the BD of the ABs was significantly lower than that of the tabular alumina aggregates. On the other hand, Figure 2a,b indicate that with the treatment temperature increasing from 110 °C to 1600 °C, the AP values of sample AB2 were 12.1%, 15.0%, 16.6%, and 15.3%. As shown in Figure 2c, the PLC values of specimens were slightly changed with an increasing AB content from 0% to 6%. The CMOR and CCS values of the samples are shown in Figure 2d,e. As revealed in Figure 2d,e, the CMOR values increased to the maximums of 3.87 MPa, 18.10 MPa, 28.70 MPa, and 36.76 MPa, respectively, and decreased afterward. The CCS value exhibited a similar trend, which was 21.1 MPa, 75.4 MPa, 116.8 MPa, and 157.9 MPa, respectively. Overall, these results demonstrate that the physical properties of the castables can be improved by introducing a certain amount of ABs, which is similar to a previous report [28].

3.3. Thermo-Mechanical Properties of the Castables

Figure 3 shows the HMOR and TSR of the specimens. As presented in Figure 3a, with increasing ABs, the HMOR value was 35.2 MPa, 37.3 MPa, 34.0 MPa, and 31.3 MPa for samples AB0, AB2, AB4, and AB6, respectively, exhibiting a similar trend to their cold strength. Figure 3b shows the correlation between the CMORst and the RSR of the castables. It can be seen that the CMORst value slightly increased from 4.64 MPa to 5.68 MPa by increasing the ABs content from 0% to 4%. The RSR values of samples AB0-AB6 were 13.74%, 13.48%, 16.36%, and 15.43%, respectively. It could be inferred that the TSR of the samples could be slightly improved by adding ABs, which was attributed to the hollow structure of the ABs buffering the thermal stress during thermal shock. Additionally, the decrease in strength led to an improvement in ductility.

3.4. Aggregate Distribution of the Castables

Figure 4 shows the digital photos and their binary black and white images of the castables. As shown in Figure 4, the ABs (marked with a yellow circle) were occupied the top area of the castables, and with the increasing ABs, the distribution of the tabular alumina aggregates tended to be more uneven. The results of the Db of the samples with different AB contents are shown in Figure 5. The slope of the regression lines for samples AB0-AB6 was 1.7352, 1.7190, 1.6010, and 1.5446, respectively. This indicates that the Db values of the tabular alumina aggregates decreased with an increase in the AB content. The study conducted by He et al. [29] showed that the Db correlated with the uniformity of the distribution of the second-phase components in the sample, where a larger Db indicated a more uniform distribution of the particles. In the two-dimensional situation, the maximum value of the Db was 2. Consequently, the addition of ABs to the castables resulted in an irregular distribution of the tabular alumina aggregates in the castables. Moreover, the uneven distribution of the tabular alumina aggregates intensified with the increasing amount of ABs in the samples. The uneven distribution of the aggregates was due to the tendency of the low-density ABs floating to the top of the samples during the vibration process, making the tabular alumina aggregates migrated upward within the sample, which can be evidently seen in Figure 4.
Figure 6 illustrates the volume ratio of the ABs in the samples. As presented in Figure 7, the volumes of the ABs were 7.0%, 13.3%, and 19.0%, respectively for sample AB2, sample AB4 and sample AB6, revealing that a significant change in the volume fraction was generated by adding lightweight ABs. Therefore, the change in the volume percentage may be resulted in an uneven distribution of the tabular alumina aggregates in the castables, which triggered a decrease in the mechanical properties of the samples. As for the samples with ABs, with the decreased Db, the CMOR, CCS, and HMOR values were decreased as well, which may be ascribed to the uneven distribution of the tabular alumina aggregates, resulting in an uneven stress distribution and thereby decreasing their cold and hot strength.

3.5. Discussion

The microstructures of fracture sample AB2 fired at different temperatures are exhibited in Figure 7. As shown in Figure 7a, it can be seen that a majority of the ABs were extracted from the matrix in the sample after firing at 1100 °C, leaving behind spherical pits and suggesting that their strength was relatively lower, which is shown in Figure 2d. The factual ABs were seen in the sample fired at 1400 °C, and some cracks were propagated through the intergranular ABs (Figure 7b), indicating that the cold strength of the samples was noticeably enhanced. As shown in Figure 7c, after firing at 1600 °C, the ABs grains exhibited strong bonding with the matrix, and crack propagation primarily occurred through the AB grains. These results demonstrate that with increases in the firing temperature from 1100 °C to 1600 °C, the interfacial bonding between the ABs and the matrices was progressively strengthened. The fracture types containing intergranular fracture and transgranular fracture of the ABs reveal that the increases in the firing temperature enhanced the interfacial bonding between the ABs and the matrix, thereby improving the cold strength of the castable.
The physical properties, HMOR, and TSR of the samples were noticeably affected by adding ABs. The AP values were increased, which may be ascribed to the hollow structure of the ABs being broken during the stirring process and some pores distributed on the shells of the ABs. The PLC values of the samples were slightly changed. The CMOR, CCS, and HMOR values of the castables were greatly impacted by introducing ABs. When the AB amount was 2 wt%, their strength was greater than that of the samples without ABs; this was owing to the spherical structure of the ABs facilitated stress buffering. With increases in the ABs from 2% to 6%, their strength decreased, which may be due to the volume fraction of the ABs increasing and the matrix fraction decreasing correspondingly, thereby decreasing the bonding mode of the ABs, tabular alumina aggregates, and the matrix. Hence, the non-uniform arrangement of the aggregates led to an inhomogeneous distribution of the strength and uneven stress distribution, consequently causing a reduction in strength [30], which is beneficial to improving the thermal shock resistance of castables with AB addition.
The SEM photos and schematic graphs of sample AB0 and sample AB4 after thermal shock are displayed in Figure 8. A trans-granular crack can be seen in sample AB0, indicating that higher thermal stress was formed after thermal shock, and therefore, the TSR of the sample without AB addition was the worst [15], which may be ascribed to their dense structure and higher strength. As for sample AB4, the propagation of the crack was impeded by the ABs (Figure 8c,d), resulting in a prolonged path for crack propagation and a reduction in the rate of crack propagation. This effect may be attributed to the hollow structure of ABs, which can effectively buffer thermal shock energy, and their spherical shape can alleviate stress concentration, thereby enhancing the thermal shock resistance of the specimens.

4. Conclusions

In this manuscript, the effects of AB addition on the properties of castables was investigated. With increasing of AB content, the apparent porosity of the castables increased and the bulk density decreased. The cold strength and hot strength firstly increased when the AB addition was 2%, and then decreased with further increasing of the Abs amount, which may be ascribed to the addition of ABs resulted in a heterogeneous distribution of the tabular alumina aggregates and finally led to the decrease in strength of the samples. The thermal shock resistance of the sample with 4% ABs was noticeably increased, which can be ascribed to the hollow structure and spherical shape of the ABs, which prolonged the crack propagation path and reduced the formation of cracks suffering from thermal shock, thereby increasing the thermal shock resistance of the castables.

Author Contributions

Conceptualization, Q.J.; Methodology, H.C.; Formal analysis, J.C. and M.S.; Investigation, H.M.; Data curation, X.S.; Writing—original draft, H.C.; Writing—review & editing, X.L. All authors have read and agreed to the published version of the manuscript.

Funding

This work was financially funded by the National Natural Science Foundation of China (grant number: 52172029) and the Collaborative Innovation Major Special Project of Zhengzhou (grant number: 20XTZX12025).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data are contained within the article.

Conflicts of Interest

Author Xingfu Shi was employed by the company Administration for Market Regulation of Xihua County. The remaining authors declare that the research was conducted in the absence of any commercial or financial relationships that could be construed as a potential conflict of interest.

References

  1. Nag, M.; Agrawal, T.; Nag, B.; Singh, B.; Biswas, S. Study and Post Mortem Analysis of Steel Ladle Porous Plug to Improve Bottom Purging Efficiency for Cleaner Steel. Eng. Fail. Anal. 2019, 101, 447–455. [Google Scholar] [CrossRef]
  2. Tripathi, P.K.; Kumar, D.S.; Sarkar, A.; Vishwanath, S.C. Optimization of Bath Mixing and Steel Cleanliness during Steel Refining through Physical and Mathematical Modeling. Sadhana-Acad. Proc. Eng. Sci. 2021, 46, 146. [Google Scholar] [CrossRef]
  3. Tan, F.; He, Z.; Jin, S.; Cai, H.; Li, B.; Li, Y.; Harmuth, H. Thermomechanical Analysis of Purging Plugs by Applying Fluid–Solid Conjugate Heat Transfer Modeling. Steel Res. Int. 2019, 90, 1900213. [Google Scholar] [CrossRef]
  4. Long, B.; Xu, G.; Buhr, A.; Jin, S.; Harmuth, H. Fracture Behaviour and Microstructure of Refractory Materials for Steel Ladle Purging Plugs in the System Al2O3-MgO-CaO. Ceram. Int. 2017, 43, 9679–9685. [Google Scholar] [CrossRef]
  5. Tan, F.; Jin, S.; He, Z.; Li, Y. Numerical Analysis of the Irreversible Behavior of Corundum Castable Purging Plugs during Service. JOM 2021, 73, 2911–2919. [Google Scholar] [CrossRef]
  6. Kumar, S.; Sarkar, R. Alumina-Spinel Castable for Steel Ladles: An Overview. Int. J. Appl. Ceram. Technol. 2023, 20, 410–423. [Google Scholar] [CrossRef]
  7. Khalil, N.M. Heat Resistance and Thermomechanical Behaviour of Ultralow and Zero Cement Castables. Adv. Appl. Ceram. 2004, 103, 37–41. [Google Scholar] [CrossRef]
  8. Zhao, F.; Ge, T.; Zhang, L.; Xu, E.; Gao, J.; Liu, X. A Novel Method for the Fabrication of Porous Calcium Hexaluminate (CA6) Ceramics Using Pre-Fired CaO/Al2O3 Pellets as Calcia Source. Ceram. Int. 2020, 46, 4762–4770. [Google Scholar] [CrossRef]
  9. Qiu, W.; Ruan, G.; Ouyang, J.; Zhao, Y.; Xu, G. Effect of Spinel Kinds on Properties of Alumina—Spinel Castables. Int. J. Appl. Ceram. Technol. 2014, 11, 993–1000. [Google Scholar] [CrossRef]
  10. Qu, J.; Ding, D.; Xiao, G.; Lei, C.; Chen, J.; Luo, J.; Zang, Y. Preparation of CaCO3 Coated Corundum Aggregates by Dip-Coating and Heat Treatment and Its Effects on the Properties and Microstructures of Al2O3–MgO Castables. Ceram. Int. 2022, 48, 5174–5186. [Google Scholar] [CrossRef]
  11. Liu, Y.; Han, B.; Zhang, T.; Yu, H.; Yan, W.; Wei, Y.; Li, N. Effect of Zirconia Particle Size on the Properties of Alumina-Spinel Castables. Ceram. Int. 2016, 42, 16961–16968. [Google Scholar] [CrossRef]
  12. Tang, H.; Li, C.; Gao, J.; Touzo, B.; Liu, C.; Yuan, W. Optimization of Properties for Alumina-Spinel Refractory Castables by CMA (CaO-MgO-Al2O3) Aggregates. Materials 2021, 14, 3050. [Google Scholar] [CrossRef]
  13. Chen, H.; Zhao, L.; He, X.; Fang, W.; Lei, Z.X.; Chen, H. The Fabrication of Porous Corundum Spheres with Core-Shell Structure for Corundum-Spinel Castables. Mater. Des. 2015, 85, 574–581. [Google Scholar] [CrossRef]
  14. Liu, G.; Jin, X.; Qiu, W.; Ruan, G.; Li, Y. The Impact of Bonite Aggregate on the Properties of Lightweight Cement-Bonded Bonite-Alumina-Spinel Refractory Castables. Ceram. Int. 2016, 42, 4941–4951. [Google Scholar] [CrossRef]
  15. Liu, J.; Zhao, L.; Jia, G.; Wang, S.; Cui, J.; Guo, H.; Liu, X.; Zhang, S.; Jia, Q. Preparation of Resin Coated Alumina Aggregate and Its Effect on the Properties of Alumina-Spinel Castables for Purging Plugs. Ceram. Int. 2022, 48, 35398–35405. [Google Scholar] [CrossRef]
  16. Geng, H.; Hu, X.; Zhou, J.; Xu, X.; Wang, M.; Guo, A.; Du, H.; Liu, J. Fabrication and Compressive Properties of Closed-Cell Alumina Ceramics by Binding Hollow Alumina Spheres with High-Temperature Binder. Ceram. Int. 2016, 42, 16071–16076. [Google Scholar] [CrossRef]
  17. Xin, Y.; Jian, Y.; Yin, H.; Tang, Y.; Yuan, H.; Liu, Y. The Influence of Alumina Bubbles on the Properties of Lightweight Corundum–Spinel Refractory. Materials 2023, 16, 5908. [Google Scholar] [CrossRef]
  18. Li, M.; Li, Y.; Ouyang, D.; Chen, R.; Li, S. The Impact of Alumina Bubble Particle Size on the Microstructure and Physical Properties of Mullite Castables. Ceram. Int. 2019, 45, 1928–1939. [Google Scholar] [CrossRef]
  19. Pentland, A.P. Fractal-Based Description of Natural Scenes. IEEE Trans. Pattern Anal. Mach. Intell. 1984, PAMI-6, 661–674. [Google Scholar] [CrossRef]
  20. Benoit, B.M. Self-Affine Fractals and Fractal Dimension. Phys. Scr. 1985, 32, 257. [Google Scholar]
  21. Tang, H.P.; Wang, J.Z.; Zhu, J.L.; Ao, Q.B.; Wang, J.Y.; Yang, B.J.; Li, Y.N. Fractal Dimension of Pore-Structure of Porous Metal Materials Made by Stainless Steel Powder. Powder Technol. 2012, 217, 383–387. [Google Scholar] [CrossRef]
  22. Wang, L.; Jin, M.; Wu, Y.; Zhou, Y.; Tang, S. Hydration, Shrinkage, Pore Structure and Fractal Dimension of Silica Fume Modified Low Heat Portland Cement-Based Materials. Constr. Build. Mater. 2021, 272, 121952. [Google Scholar] [CrossRef]
  23. Zeng, Q.; Luo, M.; Pang, X.; Li, L.; Li, K. Surface Fractal Dimension: An Indicator to Characterize the Microstructure of Cement-Based Porous Materials. Appl. Surf. Sci. 2013, 282, 302–307. [Google Scholar] [CrossRef]
  24. Fang, J.B.; Cao, Y.Q.; Chang, S.Z.; Teng, F.R.; Wu, D.; Li, A.D. Dual-Design of Nanoporous to Compact Interface via Atomic/Molecular Layer Deposition Enabling a Long-Life Silicon Anode. Adv. Funct. Mater. 2022, 32, 2109682. [Google Scholar] [CrossRef]
  25. Matsuoka, S. Fractal Character of Fracture Surfaces on Metals. Zairyo-to-Kankyo 1991, 40, 498–505. [Google Scholar] [CrossRef]
  26. Foroutan-pour, K.; Dutilleul, P.; Smith, D.L. Advances in the Implementation of the Box-Counting Method of Fractal Dimension Estimation. Appl. Math. Comput. 1999, 105, 195–210. [Google Scholar] [CrossRef]
  27. Fan, L.W.; Hu, Y.C.; Tian, T.; Yu, Z.T. The Prediction of Effective Thermal Conductivities Perpendicular to the Fibres of Wood Using a Fractal Model and an Improved Transient Measurement Technique. Int. J. Heat Mass Transf. 2006, 49, 4116–4123. [Google Scholar] [CrossRef]
  28. Xin, Y.L.; Yin, H.F.; Tang, Y.; Yuan, H.D.; Ren, X.H.; Gao, K.; Wan, Q.F.; Liu, Y.C. Effect of Alumina Bubbles with and without Al2O3 Coatings on the Performance of Lightweight Al2O3-MgAl2O4 Refractories. Int. J. Appl. Ceram. Technol. 2020, 17, 2622–2628. [Google Scholar] [CrossRef]
  29. Zhenjuan, H.; Luquan, W.; Xiaomng, P.; Zhengwei, Y.; Maolin, L.; Tianhua, Y. Research on Relationship between Value of Box Dimension in Fractal Theory and Phase Volume of the Second Phase Particles. Powder Metall. Technol. 2016, 34, 16–20. [Google Scholar]
  30. Yin, Y.; Ren, Q.; Shen, L. Study on the Effect of Aggregate Distribution on Mechanical Properties and Damage Cracks of Concrete Based on Multifractal Theory. Constr. Build. Mater. 2020, 262, 120086. [Google Scholar] [CrossRef]
Figure 1. (a,d) surficial morphology of ABs, (b,e) internal morphology of ABs, (c) XRD pattern of ABs, and (f) floating state of ABs in water.
Figure 1. (a,d) surficial morphology of ABs, (b,e) internal morphology of ABs, (c) XRD pattern of ABs, and (f) floating state of ABs in water.
Materials 17 03139 g001
Figure 2. Physical properties of the samples. (a) AP, (b) BD, (c) PLC, (d) CMOR, and (e) CCS.
Figure 2. Physical properties of the samples. (a) AP, (b) BD, (c) PLC, (d) CMOR, and (e) CCS.
Materials 17 03139 g002
Figure 3. (a) HMOR and (b) TSR of the samples with different amounts of ABs.
Figure 3. (a) HMOR and (b) TSR of the samples with different amounts of ABs.
Materials 17 03139 g003
Figure 4. Digital photos of the cross-sections and binarized pictures of the samples: (a,b) AB0, (c,d) AB2, (e,f) AB4, and (g,h) AB6. (Here, yellow circles refer to ABs).
Figure 4. Digital photos of the cross-sections and binarized pictures of the samples: (a,b) AB0, (c,d) AB2, (e,f) AB4, and (g,h) AB6. (Here, yellow circles refer to ABs).
Materials 17 03139 g004
Figure 5. The equations of linear regression of the samples: (a)AB0, (b) AB2, (c) AB4, and (d) AB6.
Figure 5. The equations of linear regression of the samples: (a)AB0, (b) AB2, (c) AB4, and (d) AB6.
Materials 17 03139 g005
Figure 6. Schematic diagram of the volume content of ABs in castables.
Figure 6. Schematic diagram of the volume content of ABs in castables.
Materials 17 03139 g006
Figure 7. The fracture morphologies of AB2 fired at (a) 1100 °C, (b) 1400 °C, and (c) 1600 °C.
Figure 7. The fracture morphologies of AB2 fired at (a) 1100 °C, (b) 1400 °C, and (c) 1600 °C.
Materials 17 03139 g007
Figure 8. SEM photos and schematic diagrams of crack propagation in the samples: (a,b) AB0 and (c,d) AB4.
Figure 8. SEM photos and schematic diagrams of crack propagation in the samples: (a,b) AB0 and (c,d) AB4.
Materials 17 03139 g008
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Chen, H.; Shi, X.; Chen, J.; Sang, M.; Ma, H.; Liu, X.; Jia, Q. Effects of Alumina Bubble Addition on the Properties of Corundum–Spinel Castables Containing Cr2O3. Materials 2024, 17, 3139. https://doi.org/10.3390/ma17133139

AMA Style

Chen H, Shi X, Chen J, Sang M, Ma H, Liu X, Jia Q. Effects of Alumina Bubble Addition on the Properties of Corundum–Spinel Castables Containing Cr2O3. Materials. 2024; 17(13):3139. https://doi.org/10.3390/ma17133139

Chicago/Turabian Style

Chen, Haonan, Xingfu Shi, Jing Chen, Mengyang Sang, Haoxuan Ma, Xinhong Liu, and Quanli Jia. 2024. "Effects of Alumina Bubble Addition on the Properties of Corundum–Spinel Castables Containing Cr2O3" Materials 17, no. 13: 3139. https://doi.org/10.3390/ma17133139

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop