Article

Modified Nanocellulose-Based Adsorbent from Sago Waste for Diclofenac Removal

by
Noorhaslin Che Su
1,
Ain Aqilah Basirun
1,
Nor Shahroon Hameed Sultan
1,
Devagi Kanakaraju
2 and
Cecilia Devi Wilfred
1,3,*
1
Centre of Research in Ionic Liquid, Universiti Teknology PETRONAS, Persiaran UTP, Seri Iskandar 32610, Perak, Malaysia
2
Faculty of Resource Science and Technology, Universiti Malaysia Sarawak, Kota Samarahan 94300, Sarawak, Malaysia
3
Fundamental and Applied Sciences Department, Universiti Teknologi PETRONAS, Persiaran UTP, Seri Iskandar 32610, Perak, Malaysia
*
Author to whom correspondence should be addressed.
Sustainability 2023, 15(7), 5650; https://doi.org/10.3390/su15075650
Submission received: 2 February 2023 / Revised: 14 March 2023 / Accepted: 15 March 2023 / Published: 23 March 2023
(This article belongs to the Section Environmental Sustainability and Applications)

Abstract

:
A nanocellulose-based adsorbent was successfully synthesized via a hydrothermal process. It was characterized by X-ray diffraction, Fourier Transform Infrared Spectroscopy, Field Emission Electron Microscopy and Brunauer–Emmett–Teller surface area analysis. Photocatalysis has the best potential to replace the conventional wastewater treatment technology through the photodegradation of organic contaminants. This study focuses on the preparation of a photocatalytic adsorbent of nanocellulose prepared from sago waste for the removal of diclofenac from industrial wastewater. Its photocatalytic activity was evaluated through the degradation of diclofenac (100 mg/L) under ultraviolet (UV) light. The effect of different loadings of TiO2 and kinetics on the photocatalytic activity was investigated. To study its removal, the experiments were carried out under UV light with different contact times ranging from 30 to 120 min at room temperature. The maximum removal percentage was found to be 57.5% for 200 µL of TiO2, and this increased up to 82.4% for 800 µL of TiO2. The maximum removal capacity was found to be 13.3 mg/g. The kinetics was well fitted with “pseudo-first order model” (PSO). Kinetic analysis using the PSO model at 100 ppm of diclofenac sodium gave a value of equilibrium adsorption capacity, qe of 13.52 mg/g. The adsorption kinetics gave a value of calculated equilibrium adsorption capacity, qe of 13.52 mg/g using different non-linear regression plots. It obeyed a pseudo-first-order reaction with the lowest AICc, RSME values of 0.56 and 0.53 and the highest correlation coefficient, R2, of 0.99. Three kinetics models were fitted for the current adsorption kinetics data, and their suitability was inferred as the following: pseudo-first-order > pseudo-second-order > Langmuir–Hinshelwood.

1. Introduction

Diclofenac (DCF) is widely used to treat fever, pain, rheumatoid arthritis, etc. [1,2,3]. The molecule is readily absorbed from the gastrointestinal tract. However, is water insoluble. DCF has been detected in µg/L in in drinking water, ground water and surface water all around the world. It can cause harmful effects on both human health and aquatic ecosystems, such as cytopathological symptoms in the gills, kidneys and liver of rainbow trout. DCF cannot be removed effectively by conventional wastewater treatment due to its stable chemical structure. Therefore, it is essential to develop more effective and sustainable treatment technologies for the removal of DCF and to treat and reuse wastewater.
Over the years, there has been increasing research into the application of nanocellulose (NC) as a smart material for water purification. Several studies have proven that NC provide greater surface areas, functional groups, water insolubility and high holding ability to extract heavy metal ions in wastewater treatment [4,5]. In addition, they offer effective and affordable treatment strategies at minimal cost.
Advanced oxidation processes (AOPs) including electrochemical oxidations, photocatalysis, photo-Fenton and ultraviolet/H2O2 have been employed to remove contaminants from wastewater. In recent years, photocatalyst technology has been a hot research area [3,6,7,8]. Heterogeneous photocatalysis is an advanced oxidation process based on light and semiconductors to generate oxidizing/reducing species dealing with environmental pollutants. Non-toxic, chemically stable titanium dioxide (TiO2) is the most widely studied as a photocatalyst [9,10,11]. Adequate photon energy (hv) irradiated onto TiO2 particle surfaces (3.2 eV (anatase form) or 3.0 eV (rutile form)) will create electron–hole pair formation (e–h+). The photonic excitation leaves behind an empty unfilled valance band, thus creating the electron–hole pair. The series of chain oxidative–reductive reactions that occur at the photon-activated surfaces is postulated as below [12]:
Photoexcitation :   TiO 2 + hv e + +   h +
Charge - carrier   trapping   of   e :   e CB e TR
Charge - carrier   trapping   of   h + :   h VB + h TR +
Electron -   hole   recombination :   e TR + h VB +   h TR + e CB + heat
Photoexcited   e   scavenging :   ( O 2 ) ads + e O 2
Oxidation   of   hydroxyls :   OH + h + OH ·
Photodegradation   by   OH   :   R H   + OH ·   R · + H 2 O
The  e TR  and  h TR +  in (Equation (4)) represent the surface-trapped valence-band electron and conduction-band hole, respectively. It was reported that these trapped carriers are usually TiO2-surface-bound and do not recombine immediately after photon excitation. In the absence of electron scavengers (Equation (4)), the photoexcited electron recombines with the valence band hole in nanoseconds with the simultaneous dissipation of heat energy. Thus, the presence of electron scavengers is vital to prolong the recombination and successful functioning of photocatalysis. Equation (5) depicts how the presence of oxygen prevents the recombination of electron–hole pairs, while allowing the formation of superoxide radical  O 2 .
NC can be applied for various approaches and possibly functions such as filters, adsorbents or membranes depending on the structure of the pore and the method of preparations. In this study, an adsorbent based on photocatalysis was prepared. The interaction of magnetite (Fe3O4) has attracted much attention with TiO2 as it influences photocatalytic activity due to its large surface area to volume ratio which offer high capacity for adsorption in wastewater treatment [13]. Thus, mixing TiO2 with magnetite and nanocellulose may provide a more sustainable use in water treatment involving adsorption [14,15] and photocatalytic activity [16].
Herein, we were able to develop a novel NC/Fe3O4/TiO2 adsorbent via a hydrothermal process. Mathematical models were used quantitatively to predict and correlate adsorption capacities/strengths and to design adsorptive processes. Modelling facilitates our understanding of biosorption dynamics, the anticipation of responses, improvements in biosorption processes, and the analysis of data [17]. Kinetics and isotherms are important in moving technology from the laboratory to the industrial scale. Kinetics describes the rate of the adsorption process, whereas isotherms represent the equilibrium connection between sorbent and adsorbent concentrations at a fixed temperature. The Akaike Information Criterion (AICc), the Root Mean-Square Error (RMSE), and the adjusted Determination Coefficient (R2) were used to determine the best-fit kinetic reaction of the present study [17].

2. Materials and Methods

2.1. Materials

Nanocellulose was prepared from sago bark waste collected from a sago industry in Sarawak. Iron (III) hexahydrate (FeCl3·6H2O), iron (II) chloride tetrahydrate (FeCl2·4H2O), trisodium citrate (Na3C6H5O7), sodium hydroxide (NaOH), titanium (IV) n- butoxide (TBOT) and ethanol were purchased from Merck. Sodium hydroxide (NaOH) and sodium acetate were purchased from Sigma Aldrich. Diclofenac (Brand: Dicloran-USP; 50 mg; pharmaceutical grade) was obtained from a local pharmacy.

2.2. Preparation of Nanocellulose Adsorbent

The methods for the preparation of the nanocellulose adsorbent are described below.

2.2.1. Isolation of Cellulose

Alkaline treatment was used to eliminate the amorphous polymer of hemicellulose and the remaining lignin [18]. The bleaching process was carried out using hydrogen peroxide. The white color of the fiber of cellulose obtained after the bleaching process indicated the successful removal of lignin and other impurities.

2.2.2. Preparation of Nanocellulose

To produce nanocellulose, 1 g of extracted cellulose was hydrolyzed with H2SO4 (40 wt.%) at 45 °C for 60 min in a ratio of 1:20. After hydrolysis, the suspension was washed repeatedly with cold deionized water. It was later centrifuged at 4000 rpm for 30 min, which gave a pearl white sediment. The slurry was further sonicated for 40 min and dried [5]. The nanocellulose powder was characterized by X-ray diffraction (XRD).

2.2.3. Synthesis of Magnetite (Fe3O4)

The Fe3O4 nanoparticles were synthesized using the chemical coprecipitation method. Fe3+ and Fe2+ with a molar ratio of 1: 2 in the form of iron (II) chloride tetrahydrate (1.00 g, 0.005 mol) and iron (III) chloride hexahydrate (2.70 g, 0.010 mol) were dissolved in 130 mL of distilled water with vigorous stirring for 2 h. Then, 30 mL of NaOH (2M) was added rapidly into the mixture, which formed a black precipitate, Fe3O4. The mixture was then heated to 60 °C for 1 h. The mixture was left to cool down to room temperature, and the magnetite was washed several times with distilled water and ethanol until a pH value of 7 was achieved. The magnetite was redispersed for 30 min in 200 mL of trisodium citrate solution (0.3 M) before being heated at 80 °C for 1 h. This was to cap the particles from further growth. The magnetite was then collected and washed with acetone to remove any remnant of trisodium citrate. Finally, the magnetite was redispersed in 100 mL of distilled water for 30 min to form a stable ferrofluid. The prepared ferrofluid was stored in a fridge (4 °C) until further use [16].

2.2.4. Synthesis of Nanocellulose/Magnetite Adsorbents (Fe3O4)

The magnetic nanocellulose/magnetite was synthesized using the hydrothermal method. First, 0.5 g of nanocellulose was dissolved in 20 mL of H2O with vigorous mechanical stirring at 80 °C in a water bath until a homogeneous viscous solution was formed. Subsequently, 0.45 g of Fe3O4 and 1.21 g of sodium acetate were added to the nanocellulose solution with vigorous agitation for 30 min at 80 °C in a water bath to form a homogeneous solution. The solution was poured into a Teflon-lined stainless-steel autoclave for hydrothermal treatment at 110, 130 and 150 °C for 4 h. It was later cooled to ambient temperature; the black precipitate product was separated by a magnet and washed several times with water and ethanol. The as-prepared samples were dried overnight at 50 °C in an oven [19].

2.2.5. Synthesis of Nanocellulose/Fe3O4/TiO2

A total of 0.10 g of nanocellulose/Fe3O4 powder was added into a 10 mL absolute ethanol solution and sonicated for ca. 20 min in an ultrasonic bath to obtain a homogenous colloidal solution. An amount of 200 μL of TBOT was added into the dispersion dropwise, and the mixture was sonicated for 15 min. It was then decanted into a vapor-phase hydrolysis apparatus (VPHA) with deionized water situated at the bottom of it to produce vapor at a raised temperature. The closed VPHA was heated to 110 °C and maintained for 5 h. Then, the VPHA was cooled to room temperature. The as-prepared powder was collected by a magnet and washed with absolute ethanol and deionized water and dried in the oven at 50 °C. The same procedure was repeated to prepare the adsorbent with various concentrations of TiO2. Table 1 describes the various types of adsorbent prepared [16,19].

2.3. Photocatalytic Reaction

Ultraviolet (UV) light photocatalytic reactions were carried out to characterize the degradations rate of diclofenac. The suspension was irradiated with an ultraviolet lamp. First, 0.1 g/L adsorbent was added to wastewater. Prior to the photocatalytic process, wastewater containing adsorbent was stirred and stored in the dark for 30 min. The diclofenac concentration was determined in the sequence of 30, 60, 90 and 120 min using a Lamba 35 UV light (Perkiin Elmer, Walthham, MA, USA). The photocatalytic activity of the adsorbent was evaluated in terms of the degradation of diclofenac in wastewater under UV-light illumination. The initial concentration of diclofenac was 100 mg/L. The suspension was stirred magnetically (200 rpm) in the dark for 30 min to reach the absorption/desorption equilibrium of the adsorbent as well as to obtain the maximum absorption of diclofenac. At the end of the first 30 min, a sample of 10 mL was taken from the wastewater by means of syringe filters (Millex Millipore, Carrigtwohill, Ireland: 0.22 µm). After the first measurement, the UV lamp was turned on, and changes in absorption under UV light were measured. A 100 W UV lamp (UVP Co., Upland, CA, USA) was used for the UV light source at the wavelength of 365 nm. The same procedure was applied after 30, 60, 90 and 120 min of UV light illumination. It is assumed that holes (h+) reacted with water molecules (H2O), which were adsorbed on the TiO2 surface, to generate hydroxyl radicals (OH.), which assisted in the degradation of the diclofenac (Figure 1).
The mechanism of diclofenac removal via photocatalysis were discussed by Martínez and team [20]. The diclofenac removal was calculated by the following Equation (8):
R   % = C 0 C 1 / C 0 ] × 100
where R is diclofenac removal percent, C0 is the initial diclofenac concentration in ppm and C1 is the concentration of diclofenac solution after irradiation in ppm.

2.4. Characterization

The nanocellulose powders’ phase compositions were identified by X-ray diffraction (XRD) equipment (D/max 2550 PC, Rigaku Co., Tokyo, Japan) using Cu Kα radiation at 40 Kv and 200 mA. The morphology was studied using a field emission scanning electron microscope (FESEM) (Model: Zeiss, Supra 55VP, Jena, Germany) equipped with an energy-dispersive X-ray and field emission scanning electron microscope (Model: Clara Tescan, Brno, Republic Czech). The samples were coated using a gold coater. The nitrogen adsorption and desorption isotherms were obtained at 77K using Autosorb -1 MP (Quantachrome, Boynton Beach, FL, USA) utilizing Barrett–Emmett–Teller calculations of pore volume and pore size (diameter) distributions from the desorption branch of the isotherm. The FTIR spectra of the samples were recorded using the PerkinElmer Spectrum in the range of 4000 cm−1 to 500 cm−1 at 4 cm−1 resolution using PerkinElmer Fourier-Transform infrared attenuated total reflection (FTIR-ATR).

2.5. Kinetic Study

The concentration of the solution of the absorbent–absorbate solution at various time intervals was determined [21,22,23]. The quantity absorbed at time t, denoted by the symbol qt (mg/g), was estimated using Equation (9). qt denotes the removal capacity by 1 g of absorbent at a certain time of exposure. It was assessed by performing an adsorption study under optimal conditions at certain time intervals until the adsorption reached an equilibrium, in this case 120 min. The non-linear regression of all kinetic models was plotted and analyzed using Curve Expert 6.0. The removal rate was assumed to be proportional to the difference between the extracted concentration and the number of accessible sites in the pseudo-first-order equation (PFO) proposed by Lagergren for solid–liquid systems [22]. The pseudo-first-order kinetic model equation is as follows:
q t = q e 1 e k 1 t
A second-order relation between the adsorption rate and the difference between saturation concentrations is proposed in the pseudo-second-order model (PSO), which implies that chemisorption is the rate-limiting step. The equation for the pseudo-second-order kinetic model is shown in Equation (10). The model is based on the adsorption capacity onto a solid phase, and the nonlinear form of PSO was initially proposed by Blanchard et al. It is expressed as:
q t = k t q e 2 t 1 + k 2   q e t
Langmuir–Hinshelwood (LH) kinetics is the most commonly used kinetic expression to explain the kinetics of catalytic processes [24]. The Langmuir–Hinshelwood expression that explains the kinetics of catalytic systems is given by:
q t = d C d t = k t K C 1 + K C
where  q t  represents the rate of reaction that changes with time.
The model involves two steps: the adsorption of reactants onto the catalyst surface and reaction of the adsorbed species. The rate of the overall reaction is determined by the rate of the slower step.
The term r in Equation (11) was represented in terms of the initial reaction rate, r0, as a function of the initial diclofenac concentration, C0, or in terms of Ce, where Ce is the equilibrium diclofenac concentration in solution after the completion of dark experiments. The initial rate of the reaction as a function of C0 and Ce is given by Equations (12) and (13), respectively:
q t = k t K C 0 1 + K C 0
q t = k t K C e 1 + K C e

2.6. Statistical Analysis

For all models tested in this study, statistical discriminatory tests such as Root-Mean-Square Error (RMSE), corrected AICc (Akaike Information Criterion), accuracy factor (AF) and bias factor (BF) and adjusted coefficient of determination (R2) were utilized in this work. All the parameter estimations were made using CurveExpert 6.0.
The RMSE was calculated according to Equation (14) where n is experimental data points, Obi and Pdi are the experimental and predicted data, respectively, while p is parameter numbers [17].
R M S E = i = 1 n P d i O b i 2 n p
The Akaike Information Criterion (AIC) AICc, which is based on the information theory [23], is calculated as follows (Equation (15)):
A I C c = 2 p + n ln R S S n + 2 p + 1 + 2 p + 1 p + 2 n p 2
Further error function analyses are the Accuracy Factor (AF) and Bias Factor (BF) (Equations (16) and (17)).
Bias factor = 10 i = 1 n log P d i / O b i n
Accuracy   factor   = 10 i = 1 n log P d i / O b i n

3. Results and Discussions

Figure 2 shows the XRD peak for raw sago and nanocellulose. The crystallinity index, CrI for each sample, was determined based on Equation (18) [25]:
C r I = I   002 I a m I a m
where  I   002  is the maximum intensity of the (0 0 2) lattice diffraction peak and  I a m  is the intensity scattered by the amorphous part of the sample. The diffraction peak for plane (0 0 2) is located at a diffraction angle around 2θ = 22°, and the intensity scattered by the amorphous part is measured as the lowest intensity at a diffraction angle around 2θ = 18°. The crystallinity index for raw sago and nanocellulose is 23% and 73%, respectively. The crystallinity of nanocellulose demonstrates higher crystallinity because of the efficient removal of the amorphous parts by the cleavage of glycosidic linkages releasing crystallites [8].
Figure 3 shows the XRD peak for nanocellulose/Fe3O4 prepared at different temperatures. The peaks at 2θ = 30.1°,35.3°, 43° and 53.3° and 62.7° stand for [(220), (311), (400), (422) and (440)] which are consistent with the main phases of the magnetite (Fe3O4)—JCPDS card no. 019–0629 [19]. The peaks at 2θ = 18.2°, 30.5°, 35.7°, 43.4°, 53.55°, 57.5° and 62.9° stand for the (111), (220), (311), (400), (422), (511) and (440) planes, representing the nanocellulose/Fe3O4. These peaks appeared to have weak intensities due to the interaction of magnetite and nanocellulose [26]. The nanocellulose/Fe3O4 prepared at 130 °C was further added with TiO2.
Figure 4 shows the XRD peaks for nanocellulose/Fe3O4 and nanocellulose/Fe3O4/TiO2 magnetite adsorbent. The peaks at 2θ = 30.1°, 35.3°, 43°, 53.3° and 62.7° which stand for [(220), (311), (400), (422) and (440)] are consistent with the main phases of the magnetite (Fe3O4)—JCPDS card no. 019-0629 [19]. The peaks at 2θ = 25.68°, 38.47°, 48.13° and 54.55° which stand for the (101), (103), (200) and (105) refer to anatase phase of TiO2 and demonstrate the formation of well-crystallized TiO2 (JCPDS card no 01-0562) [27]. The XRD results demonstrate that the crystalline and anatase Fe3O4 and TiO2, respectively, coexisted in the adsorbent sample.
Figure 5 shows the comparison of the FTIR spectra range of the prepared nanocellulose, Fe3O4, NC/Fe3O4, Ads-1, Ads-2 and Ads-3. The spectrum shows the appearance peaks at 1064, 1639 and 2893 cm−1 which represent -C-O-, C=O and -C-H stretching, respectively [28]. Meanwhile, the Fe3O4 spectrum shows peaks at 542 and 1647 cm−1 which represent Fe-O stretching and C=O, respectively [29]. Ads-1 shows the presence of nanocellulose and magnetite Fe3O4 peaks. A similar pattern was observed for Ads-2 and Ads-3. The wide absorption band around 3600–3000 cm−1 that appeared in all samples was attributed to the stretching vibration of −OH from the hydroxyl group originated from the free water molecules on the adsorbent surfaces [28,30].
Further analysis was carried out using FESEM to compare the surface morphologies of the synthesized adsorbent. Figure 5 demonstrates that NC/Fe3O4 appeared to have smoother appearances compared to NC/Fe3O4/TiO2 (200 µL), which showed rougher surfaces. The rougher surfaces allowed more diclofenac molecules to be absorbed onto them. White particles (marked red) on the NC/Fe3O4/TiO2 surface were identified as TiO2 particles. This is supported by the EDX results. This finding shows that TiO2 particles were well dispersed on the NC/Fe3O4 surface. Figure 6c shows the FESEM mapping result of Ads-1. This further confirms the presence of TiO2 along with carbon (C) and iron (Fe).
The surface area, pore volume and pore diameter of prepared adsorbents were determined using BET. Based on Table 2, the prepared adsorbents could be classified in the category of mesoporous as their pore sizes were in the range of 2–10 nm. With the addition of more TiO2 from 200 µL to 400 µL, the BET surface area increased. However, with the addition of more TiO2 up to 800 µL, the surface area decreased, as TiO2 tends to agglomerate and cumulate in pores [27].
Studies on the effect of varying the adsorbent dosage of TiO2 in NC/Fe3O4/TiO2 from 200 µL to 800 µL on the DCF removal within a 120 min reaction were carried out. Upon UV irradiation, DCF removal showed 57% with 200 µL TiO2 loading. The removal percentages displayed no significant changes (57.4%) with the addition of a TiO2 dosage up to 400 µL. However, the removal of diclofenac increased up to 82% with the addition of an 800 µL TiO2 dosage (Figure 7). This signifies that 800 µL pf TiO2 is the best amount to promote maximum UV light absorption and transfer the charge carriers to the surface for photocatalytic treatment. The OH radicals that were produced in the photocatalytic process oxidized the DCF organic pollutant to intermediates/degradation products and finally to complete mineralization. The degradation pathway of DCF is reported to include hydroxylation, the cleavage of the N-H bond, dehalogenation and aromatic ring opening [10].
Figure 8 shows the removal percentage of diclofenac as a function of time with different loadings of TiO2. In the first 30 min in the dark, the removal of diclofenac increased up to 50% for 200 µL and 400 µL loadings of TiO2. This shows that the presence of nanocellulose and magnetite in the adsorbent system facilitated the DCF removal through the adsorption process [16]. It is known that cellulose and magnetite are good adsorbents [31]. This shows that NC/Fe3O4/TiO2 could remove 50% of DCF in dark conditions predominantly by the adsorption process. Upon UV irradiation from 30 min to 120 min, although the TiO2 dosage increased from 200 to 400 µL, only a very small increment in DCF was removed. The removal of DCF was not greatly impacted by increasing the dosage of TiO2 from 200 to 400 µL but was favored by the adsorption process and a minimum amount by photocatalytic activity. This finding corroborates with those reported by Kanakaraju et al. [16]. However, with a higher loading of TiO2 at 800 µL, the removal percentage of diclofenac was seen to increase up to 87%, indicating photocatalytic activity dominates the removal of DCF. There could be more •OH radicals formed that could have aided in the removal of diclofenac. The adsorption and photocatalytic reaction behavior can be further discussed through kinetic analysis prediction.
Kinetic analysis was analyzed using three models which were pseudo-first-order (PFO), pseudo-second-order (PSO) and Langmuir–Hinshelwood (LH) kinetic (Figure 8). Since the linearization of nonlinear data disturbs the data’s error structure, this makes it harder to assess uncertainty, which is often reported as the 95% confidence interval range [20]. Hence, non-linear regression is preferable for kinetic model fitting since it is conducted on the same abscissa with a linear regression plot, showing more accurate calculations. Figure 9a,b depict the experimental and calculated data plot on pseudo-first and pseudo-second kinetic models, respectively, while Figure 9c shows the Langmuir–Hinshelwood (L-H) model with an unfit data plot. This L-H plot is abundantly being studied in photocatalysis study. However, for the study of batch removal, it has limited applications in heterogeneous catalytic systems since it usually offers negative-order kinetics, which cause erroneous results to be obtained as the kinetic rate parameters estimated at intrinsic kinetic conditions fail to predict the reaction rate when mass transport limitation also plays a role [32]. Another limitation of the Langmuir–Hinshelwood mechanism is that it does not account for the possibility of multiple reaction pathways, which can lead to different reaction products. Additionally, the assumption of random reactions between adsorbed species may not always be accurate, as some surface structures may favor certain reaction pathways over others. Lastly, the Langmuir–Hinshelwood mechanism assumes that the catalyst surface is homogeneous, while real catalysts often have heterogeneous surface structures that can affect the reaction kinetics. A previous recent finding claims that the validity of the L-H model in photocatalytic reaction could be a misinterpretation, and without proper experimental evidence, it is dubious [32,33].
Considering the statistical indicators, pseudo-first-order is more accurate in describing the diclofenac removal kinetic profiles than PSO and LH based on error functions analysis with the lowest SSE and AICc, with an R2 nearest to 1.0 (Table 3). Kinetic analysis using the PSO model at 100 ppm of diclofenac sodium gives a value of equilibrium adsorption capacity, with a qe of 13.52 mg g−1 (Table 4). It was inferred that the three kinetics models discovered to be suitable for fitting the current adsorption kinetics data are as follows: pseudo-first-order > pseudo-second-order > Langmuir–Hinshelwood. As far as diclofenac removal is concerned, the PFO was the best model for the crosslinked soy polysaccharide-based hydrogel nanostructure [34,35,36].
The pseudo-first-order model was utilized to fit data for all TiO2 loadings, and the data showed excellent agreement with the pseudo-first-order equation (Figure 10) with all regressed lines showing correlation coefficients, R2 > 0.99. As a result, it is reasonable to conclude that the process is pseudo-first-order rather than pseudo-second-order or Langmuir–Hinshelwood. It is also possible that adsorption happens in nature as physisorption, which portray the physical adsorption between two-phase system bulk that is reversible in nature [37,38,39]. The present study also shows accordance with the findings of a previous analysis of adsorption using a ZnO-chitosan nanocomposite as the nanocellulose component [40].

4. Conclusions

We developed an adsorbent comprising nanocellulose that was obtained from sago waste. Fe3O4/TiO2 was added to the nanocellulose to give a photocatalytic adsorbent. The system was able to remove diclofenac from industrial wastewater with 57.5% with 200 µL of TiO2, and this increased up to 82.4% with 800 µL of TiO2. The maximum removal capacity was found to be 13.3 mg/g. The kinetics was well fitted with the pseudo-first-order model, which gave a qe of 13.52 mg/g. The statistical analyses showed the lowest AICc and RSME values of 0.56 and 0.53, respectively, and the highest correlation coefficient, R2, of 0.99. This research has demonstrated the synergistic interaction of adsorption and photocatalysis reactions for environmental pollutant removal.

Author Contributions

Conceptualization, N.C.S. and A.A.B.; methodology, D.K. and N.S.H.S.; formal analysis, N.C.S. and A.A.B.; writing—original draft preparation, N.C.S.; writing—review and editing, N.C.S. and A.A.B.; supervision, C.D.W.; funding acquisition, C.D.W. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Yayasan Universiti Teknologi PETRONAS Fundamental Research Grant (YUTP), 015LC0-256.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data is contained within the article.

Acknowledgments

The authors would like to thank Yayasan Universiti Teknologi PETRONAS Fundamental Research Grant (YUTP), 015LC0-256 for the project funding and the technical support provided by Mohd Yunus Abd Shukor, Biochemistry Department, Faculty of Biotechnology & Biomolecular Sciences, Universiti Putra Malaysia.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Benotti, M.J.; Trenholm, R.A.; Vanderford, B.J.; Holady, J.C.; Stanford, B.D.; Snyder, S.A. Pharmaceuticals and endocrine disrupting compounds in u.s. drinking water. Environ. Sci. Technol. 2009, 43, 597–603. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  2. Hanif, H.; Waseem, A.; Kali, S.; Qureshi, N.A.; Majid, M.; Iqbal, M.; Ur-Rehman, T.; Tahir, M.; Yousaf, S.; Iqbal, M.M.; et al. Environmental risk assessment of diclofenac residues in surface waters and wastewater: A hidden global threat to aquatic ecosystem. Environ. Monit. Assess. 2020, 192, 204. [Google Scholar] [CrossRef] [PubMed]
  3. Steven, T.; Nawaz, R.; Sahrin, N.T.; Lee, K.M.; Bianchi, C.L.; Chong, F.K. H2O2-assisted Sonophotocatalytic Degradation of Diclofenac Using a Visible Light-Active Flower-like Micron-Sized TiO2 Photocatalyst. Malays. J. Chem. 2021, 23, 108–125. [Google Scholar] [CrossRef]
  4. Abou-Zeid, R.E.; Khiari, R.; El-Wakil, N.; Dufresne, A. Current State and New Trends in the Use of Cellulose Nanomaterials for Wastewater Treatment. Biomacromolecules 2018, 20, 573–597. [Google Scholar] [CrossRef]
  5. Reshmy, R.; Thomas, D.; Philip, E.; Paul, S.A.; Madhavan, A.; Sindhu, R.; Binod, P.; Pugazhendhi, A.; Sirohi, R.; Tarafdar, A.; et al. Potential of nanocellulose for wastewater treatment. Chemosphere 2021, 281, 130738. [Google Scholar] [CrossRef]
  6. Addamo, M.; Augugliaro, V.; Di Paola, A.; Garcia-Lopez, E.; Loddo, V.; Marci, G.; Molinari, R.; Palmisano, L.; Schiavello, M. Preparation, Characterization, and Photoactivity of Polycrystalline Nanostructured TiO2 Catalysts. J. Phys. Chem. B 2004, 108, 3303–3310. [Google Scholar] [CrossRef]
  7. Zhang, S.; Guo, S.; Li, A.; Liu, D.; Sun, H.; Zhao, F. Low-cost bauxite residue-MoS2 possessing adsorption and photocatalysis ability for removing organic pollutants in wastewater. Sep. Purif. Technol. 2022, 283, 120144. [Google Scholar] [CrossRef]
  8. Pan, Y.; Zhang, Y.; Huang, Y.; Jia, Y.; Chen, L. Enhanced photocatalytic oxidation degradability for real cyanide wastewater by designing photocatalyst GO/TiO2/ZSM-5: Performance and mechanism research. Chem. Eng. J. 2022, 428, 131257. [Google Scholar] [CrossRef]
  9. Leong, S.; Razmjou, A.; Wang, K.; Hapgood, K.; Zhang, X.; Wang, H. TiO2 based photocatalytic membranes: A review. J. Membr. Sci. 2014, 472, 167–184. [Google Scholar] [CrossRef]
  10. Kanakaraju, D.; Motti, C.A.; Glass, B.D.; Oelgemoller, M. Photolysis and TiO2-catalysed degradation of diclofenac in surface and drinking water using circulating batch photoreactors. Environ. Chem. 2014, 11, 51–62. [Google Scholar] [CrossRef] [Green Version]
  11. Mu, R.; Xu, Z.; Li, L.; Shao, Y.; Wan, H.; Zheng, S. On the photocatalytic properties of elongated TiO2 nanoparticles for phenol degradation and Cr(VI) reduction. J. Hazard. Mater. 2010, 176, 495–502. [Google Scholar] [CrossRef] [PubMed]
  12. Chong, M.N.; Jin, B.; Chow, C.W.K.; Saint, C. Recent developments in photocatalytic water treatment technology: A review. Water Res. 2010, 44, 2997–3027. [Google Scholar] [CrossRef]
  13. Villa, S.; Caratto, V.; Locardi, F.; Alberti, S.; Sturini, M.; Speltini, A.; Maraschi, F.; Canepa, F.; Ferretti, M. Enhancement of TiO2 NPs Activity by Fe3O4 Nano-Seeds for Removal of Organic Pollutants in Water. Materials 2016, 9, 771. [Google Scholar] [CrossRef] [Green Version]
  14. Zaidi, N.A.H.M.; Lim, L.B.L.; Usman, A.; Kooh, M.R.R. Efficient adsorption of malachite green dye using Artocarpus odoratissimus leaves with artificial neural network modelling. Desalin. Water Treat. 2018, 101, 313–324. [Google Scholar] [CrossRef]
  15. Rahimi Kooh, M.R.; Thotagamuge, R.; Chau, Y.-F.C.; Mahadi, A.H.; Lim, C.M. Machine learning approaches to predict adsorption capacity of Azolla pinnata in the removal of methylene blue. J. Taiwan Inst. Chem. Eng. 2022, 132, 104134. [Google Scholar] [CrossRef]
  16. Kanakaraju, D.; Lim, Y.-C.; Pace, A. Magnetic hybrid TiO2/Alg/FeNPs triads for the efficient removal of methylene blue from water. Sustain. Chem. Pharm. 2018, 8, 50–62. [Google Scholar] [CrossRef]
  17. Hami, H.K.; Ruba, F.A.; Amel, S.M.; Asma, A.M. An overview of using error function in adsorption isotherm modeling. Muthanna J. Pure Sci. (MJPS) 2021, 8, 22–30. [Google Scholar] [CrossRef]
  18. Naduparambath, S.; Purushothaman, E. Sago seed shell: Determination of the composition and isolation of microcrystalline cellulose (MCC). Cellulose 2016, 23, 1803–1812. [Google Scholar] [CrossRef]
  19. Aghamali, A.; Khosravi, M.; Hamishehkar, H.; Modirshahla, N.; Behnajady, M.A. Preparation of novel high performance recoverable and natural sunlight-driven nanocomposite photocatalyst of Fe3O4/C/TiO2/N-CQDs. Mater. Sci. Semicond. Process. 2018, 87, 142–154. [Google Scholar] [CrossRef]
  20. Martínez, C.; Canle, L.M.; Fernández, M.I.; Santaballa, J.A.; Faria, J. Aqueous degradation of diclofenac by heterogeneous photocatalysis using nanostructured materials. Appl. Catal. B Environ. 2011, 107, 110–118. [Google Scholar] [CrossRef]
  21. Subramanyam, B.; Das, A. Linearised and non-linearised isotherm models optimization analysis by error functions and statistical means. J. Environ. Health Sci. Eng. 2014, 12, 92. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  22. Azizian, S. Kinetic models of sorption: A theoretical analysis. J. Colloid Interface Sci. 2004, 276, 47–52. [Google Scholar] [CrossRef]
  23. Basirun, A.A.; Khudri, M.A.M.R.S.; Yasid, N.A.; Othman, A.R.; Johari, W.L.W.; Shukor, M.Y.; Halmi, M.I.E. Kinetic Analysis for the Removal of Copper Using Durvillaea antarctica. J. Environ. Microbiol. Toxicol. 2019, 7, 32–35. [Google Scholar] [CrossRef]
  24. Kumar, M.; Tamilarasan, R. Kinetics, equilibrium data and modeling studies for the sorption of chromium by Prosopis juliflora bark carbon. Arab. J. Chem. 2017, 10, S1567–S1577. [Google Scholar] [CrossRef] [Green Version]
  25. Segal, L.; Creely, J.J.; Martin, A.E., Jr.; Conrad, C.M. An Empirical Method for Estimating the Degree of Crystallinity of Native Cellulose Using the X-Ray Diffractometer. Text. Res. J. 1959, 29, 786–794. [Google Scholar] [CrossRef]
  26. Zheng, J.; Wu, Y.; Zhang, Q.; Li, Y.; Wang, C.; Zhou, Y. Direct liquid phase deposition fabrication of waxberry-like magnetic Fe3O4@TiO2 core-shell microspheres. Mater. Chem. Phys. 2016, 181, 391–396. [Google Scholar] [CrossRef]
  27. Shi, F.; Li, Y.; Zhang, Q.; Wang, H. Synthesis of Fe3O4/C/TiO2 magnetic photocatalyst via vapor phase hydrolysis. Int. J. Photoenergy 2012, 2012, 365401. [Google Scholar] [CrossRef] [Green Version]
  28. Salamat, S.; Younesi, H.; Bahramifar, N. Synthesis of magnetic core–shell Fe3O4@TiO2 nanoparticles from electric arc furnace dust for photocatalytic degradation of steel mill wastewater. RSC Adv. 2017, 7, 19391–19405. [Google Scholar] [CrossRef] [Green Version]
  29. Gopalakannan, V.; Viswanathan, N. One pot synthesis of metal ion anchored alginate–gelatin binary biocomposite for efficient Cr(VI) removal. Int. J. Biol. Macromol. 2016, 83, 450–459. [Google Scholar] [CrossRef]
  30. Ben Hammouda, S.; Adhoum, N.; Monser, L. Synthesis of magnetic alginate beads based on Fe3O4 nanoparticles for the removal of 3-methylindole from aqueous solution using Fenton process. J. Hazard. Mater. 2015, 294, 128–136. [Google Scholar] [CrossRef]
  31. Wei, J.; Yang, Z.; Sun, Y.; Wang, C.; Fan, J.; Kang, G.; Zhang, R.; Dong, X.; Li, Y. Nanocellulose-based magnetic hybrid aerogel for adsorption of heavy metal ions from water. J. Mater. Sci. 2019, 54, 6709–6718. [Google Scholar] [CrossRef]
  32. Gangwal, V.; Van Der Schaaf, J.; Kuster, B.; Schouten, J. The effect of mass transport limitation on the estimation of intrinsic kinetic parameters for negative order reactions. Appl. Catal. A Gen. 2004, 274, 275–283. [Google Scholar] [CrossRef]
  33. Lazar, M.A.; Varghese, S.; Nair, S.S. Photocatalytic Water Treatment by Titanium Dioxide: Recent Updates. Catalysts 2012, 2, 572–601. [Google Scholar] [CrossRef] [Green Version]
  34. Anirudhan, T.; Rejeena, S. Photocatalytic degradation of eosin yellow using poly (pyrrole-co-aniline)-coated TiO2/nanocellulose composite under solar light irradiation. J. Mater. 2015, 2015, 636409. [Google Scholar] [CrossRef] [Green Version]
  35. Rathod, M.; Moradeeya, P.G.; Haldar, S.; Basha, S. Nanocellulose/TiO2 composites: Preparation, characterization and application in the photocatalytic degradation of a potential endocrine disruptor, mefenamic acid, in aqueous media. Photochem. Photobiol. Sci. 2018, 17, 1301–1309. [Google Scholar] [CrossRef]
  36. Yue, Y.; Shen, S.; Cheng, W.; Han, G.; Wu, Q.; Jiang, J. Construction of mechanically robust and recyclable photocatalytic hydrogel based on nanocellulose-supported CdS/MoS2/Montmorillonite hybrid for antibiotic degradation. Colloids Surf. A Physicochem. Eng. Aspects 2022, 636, 128035. [Google Scholar] [CrossRef]
  37. Kumar, K.V.; Porkodi, K.; Rocha, F. Langmuir–Hinshelwood kinetics—A theoretical study. Catal. Commun. 2008, 9, 82–84. [Google Scholar] [CrossRef]
  38. Tran, H.N.; You, S.; Hosseini-Bandegharaei, A.; Chao, H. Mistakes and inconsistencies regarding adsorption of contaminants from aqueous solutions: A critical review. Water Res. 2017, 120, 88–116. [Google Scholar] [CrossRef]
  39. Kopinke, F.-D.; Georgi, A.; Goss, K.-U. Comment on “Mistakes and inconsistencies regarding adsorption of contaminants from aqueous solution: A critical review, published by Tran et al. [Water Research 120, 2017, 88–116]”. Water Res. 2018, 129, 520–521. [Google Scholar] [CrossRef]
  40. Zango, Z.U.; Dennis, J.O.; Aljameel, A.I.; Usman, F.; Mohammed Ali, M.K.; Abdulkadir, B.A.; Algessair, S.; Aldaghri, O.A.; Ibnaouf, K.H. Effective removal of methylene blue from simulated wastewater using ZnO-chitosan nanocomposites: Optimization, kinetics, and Isotherm studies. Molecules 2022, 27, 4746. [Google Scholar] [CrossRef]
Figure 1. The schematic diagram of the photocatalytic degradation of the organic compound [9].
Figure 1. The schematic diagram of the photocatalytic degradation of the organic compound [9].
Sustainability 15 05650 g001
Figure 2. XRD peak for raw sago and nanocellulose.
Figure 2. XRD peak for raw sago and nanocellulose.
Sustainability 15 05650 g002
Figure 3. XRD peak for Fe3O4/Nanocellulose prepared at different temperatures.
Figure 3. XRD peak for Fe3O4/Nanocellulose prepared at different temperatures.
Sustainability 15 05650 g003
Figure 4. XRD peaks for nanocellulose/Fe3O4 and nanocellulose/Fe3O4/TiO2.
Figure 4. XRD peaks for nanocellulose/Fe3O4 and nanocellulose/Fe3O4/TiO2.
Sustainability 15 05650 g004
Figure 5. The FTIR spectra of nanocellulose, Fe3O4 (magnetite), nanocellulose + magnetite and the prepared adsorbent (Ads-1, Ads-2 and Ads-3).
Figure 5. The FTIR spectra of nanocellulose, Fe3O4 (magnetite), nanocellulose + magnetite and the prepared adsorbent (Ads-1, Ads-2 and Ads-3).
Sustainability 15 05650 g005
Figure 6. The FESEM of (a) NC/ Fe3O4 (b) Ads-1 and (c) mapping results of Ads-1.
Figure 6. The FESEM of (a) NC/ Fe3O4 (b) Ads-1 and (c) mapping results of Ads-1.
Sustainability 15 05650 g006
Figure 7. Percentage of diclofenac removal with different loadings of TiO2.
Figure 7. Percentage of diclofenac removal with different loadings of TiO2.
Sustainability 15 05650 g007
Figure 8. Percentage of diclofenac removal with contact time.
Figure 8. Percentage of diclofenac removal with contact time.
Sustainability 15 05650 g008
Figure 9. Kinetics of 100 ppm diclofenac removal using photocatalysis reaction (800 µL of TiO2) as modeled using the pseudo-first-order (a), pseudo-second-order (b) and Langmuir–Hinshelwood (c) models (data at time zero are omitted due to natural logarithm transformation restriction).
Figure 9. Kinetics of 100 ppm diclofenac removal using photocatalysis reaction (800 µL of TiO2) as modeled using the pseudo-first-order (a), pseudo-second-order (b) and Langmuir–Hinshelwood (c) models (data at time zero are omitted due to natural logarithm transformation restriction).
Sustainability 15 05650 g009
Figure 10. Experimental data versus calculated data (line) on pseudo-first-order kinetic analysis of TiO2 loading effect on removal of sodium diclofenac sodium under photocatalysis.
Figure 10. Experimental data versus calculated data (line) on pseudo-first-order kinetic analysis of TiO2 loading effect on removal of sodium diclofenac sodium under photocatalysis.
Sustainability 15 05650 g010
Table 1. Synthesized adsorbent with various dosages of TiO2.
Table 1. Synthesized adsorbent with various dosages of TiO2.
AdsorbentSample Code
Nanocellulose/Fe3O4NC/Fe3O4
Nanocellulose/Fe3O4/TiO2 (200 µL)Ads-1
Nanocellulose/Fe3O4/TiO2 (400 µL)Ads-2
Nanocellulose/Fe3O4/TiO2 (800 µL)Ads-3
Table 2. The results of BET analyses for the prepared adsorbent.
Table 2. The results of BET analyses for the prepared adsorbent.
AdsorbentBET Surface Area
(m2/g)
Pore Volume
(cm3/g)
Pore Diameter
(nm)
Ads-174.870.12826.853
Ads-2160.650.1676.354
Ads-3 103.390.1556.011
Table 3. Statistical analysis for removal of sodium diclofenac using 800 µL TiO2 loading amount in photocatalytic reaction.
Table 3. Statistical analysis for removal of sodium diclofenac using 800 µL TiO2 loading amount in photocatalytic reaction.
ModelRMSER2AICc
Pseudo-1st-order0.5260.9970.558
Pseudo-2nd-order1.2710.9715.064
Langmuir-Hinshelwood3.3440.63128.47
Table 4. Model constants for the kinetics study of removal of sodium diclofenac.
Table 4. Model constants for the kinetics study of removal of sodium diclofenac.
ModelAdsorption Capacity, qe (mg/g)Constant, k (95% Confidence Interval)
Pseudo-1st-order13.520.04 (0.023 to 0.05)
Pseudo-2nd-order17.230.002(0.0065 to 0.004059)
L-H1.330.07(0.0032 to 0.0562)
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Che Su, N.; Basirun, A.A.; Hameed Sultan, N.S.; Kanakaraju, D.; Wilfred, C.D. Modified Nanocellulose-Based Adsorbent from Sago Waste for Diclofenac Removal. Sustainability 2023, 15, 5650. https://doi.org/10.3390/su15075650

AMA Style

Che Su N, Basirun AA, Hameed Sultan NS, Kanakaraju D, Wilfred CD. Modified Nanocellulose-Based Adsorbent from Sago Waste for Diclofenac Removal. Sustainability. 2023; 15(7):5650. https://doi.org/10.3390/su15075650

Chicago/Turabian Style

Che Su, Noorhaslin, Ain Aqilah Basirun, Nor Shahroon Hameed Sultan, Devagi Kanakaraju, and Cecilia Devi Wilfred. 2023. "Modified Nanocellulose-Based Adsorbent from Sago Waste for Diclofenac Removal" Sustainability 15, no. 7: 5650. https://doi.org/10.3390/su15075650

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop