Next Article in Journal
Polymeric Terbium(III) Squarate Hydrate as a Luminescent Magnet
Next Article in Special Issue
Simple Approach to Medical Grade Alumina and Zirconia Ceramics Surface Alteration via Acid Etching Treatment
Previous Article in Journal
Incorporation of Iron(II) and (III) in Hydroxyapatite—A Theoretical Study
Previous Article in Special Issue
Green Synthesis of Ge1−xSnx Alloy Nanoparticles for Optoelectronic Applications
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

The Effects of Li+ Doping on Structure and Upconversion Luminescent Properties for Bi3.46Ho0.04Yb0.5Ti3O12: xLi Phosphors

1
Guangxi Key Laboratory of Processing for Non-Ferrous Metals and Featured Materials, MOE Key Laboratory of New Processing Technology for Non-Ferrous Metals and Materials, Guangxi University, Nanning 530004, China
2
School of Resources, Environment and Materials, Guangxi University, Nanning 530004, China
*
Author to whom correspondence should be addressed.
Crystals 2021, 11(10), 1220; https://doi.org/10.3390/cryst11101220
Submission received: 20 September 2021 / Revised: 5 October 2021 / Accepted: 5 October 2021 / Published: 9 October 2021

Abstract

:
A series of novel Li+ doped Bi3.46Ho0.04Yb0.5Ti3O12 (BHYTO: xLi, 0 ≤ x ≤ 0.15) upconversion phosphors were prepared through a sol-gel-sintering method. There exist three emission bands centered at 545 nm, 658 nm, and 756 nm in the upconversion emission spectra at 980 nm excitation, corresponding to energy transitions of 5F4/5S2 → 5I8, 5F5 → 5I8 and 5F4/5S2 → 5I7 of Ho3+, and the upconversion emission intensity of BHYTO: 0.05Li is about 2.2 times stronger than that of BHYTO samples. The luminescent lifetime of the strongest emission (545 nm) is in the range of 45.25 to 65.99 μs for the different BHYTO: xLi phosphors. The energy transfers during the upconversion pumping process from Yb3+ to Ho3+ are mainly responsible for all the emissions, each belonging to a double-photon process. Li+ mainly entered into the interspace sites or occupied Bi3+ sites in Bi4Ti3O12 host during the fabrication process according to its dosage, and the possibility is very low for Li+ to take part in the energy transfer process directly due to its lack of matching levels with 4f of Ho3+ and Yb3+. However, Li+ doping can not only increase the size of crystal grains to improve crystallinity through XRD analysis, but also reduced oxygen vacancies to decrease the number of quenching centers through XPS analysis. The improved crystallinity and reduced quenching centers are proposed to be the main causes for the enhanced upconversion luminescence of the Li+ doped BHYTO phosphor.

1. Introduction

Rare earth (RE) doped upconversion (UC) phosphors played important roles in LED [1], display [2], biological image [3], laser [4], and optical fiber [5], attracting a lot of interests to develop novel optical materials. Bi4Ti3O12 (BTO) based materials with an Aurivillius structure have been studied intensively for a long time due to their good electric properties [6], and almost all RE3+ doping has positive effects on improving its ferroelectricity of BTO [7]. Following that, the excellent photoluminescence was observed in the BTO based multifunctional materials, such as Er3+, Tm3+, Ho3+, Yb3+ single doped, or co-doped BTO phosphors [8]. Recently, an efficient UC phosphor of Ho3+–Yb3+ co-doped Bi3.46Ho0.04Yb0.5Ti3O12 (BHYTO) powder was reported [9]. There are three main reasons to contribute BTO to be a good optical host for photoluminescence: (1) RE3+ ions have a large solid solubility to substitute Bi3+ sites and can disperse evenly in BTO crystal lattice due to similar ionic radius and the same valence state as Bi3+ [10], and (2) they can stabilize oxygen in BTO crystal lattice and reduce oxygen vacancy [11], and (3) BTO has a low phonon energy and good physical and chemical stability [12].
Although a lot of RE3+ doped phosphors were designed and invented so far, only a few of them obtained practical applications because most of them have a lower luminescence efficiency. So the research on how to improve luminescence efficiency through a simple method has a higher value than only to find a novel phosphor. Doping of assistant ions in phosphors has been considered to be an efficient and important way in improving luminescence property [13]. Li+ was the most used assistant ion in either down shifting or upconversion RE phosphors. It can enter into the host crystal lattice of these phosphors easily without destroying the original crystal structure since it has a small ion radius and simple electron configuration. However, the enhanced amplitude and initial causes for luminescence improvement in these RE phosphors were usually different, even for the same phosphor fabricated with different methods. For examples, the emission intensities of Li+ doped CaMoO4: Er3+, Yb3+ [14], Gd2O3: Yb3+, Ho3+ [15], and Y2O3: Eu3+ [16] were reported to be 83, 10, and 1.2 times higher than those of phosphors without Li+ doping. At present, there are many proposals to illustrate the role of Li+ in the process of luminescence enhancement, such as local crystal field distortion [14], charge compensation [17], change in morphology [18], and improved crystallinity and increased grain size [19]. However, some of these proposals were short of data support or not discussed in detail.

2. Experiment

In the formula of Bi3.46Ho0.04Yb0.5Ti3O12: xLi (x = 0, 0.02, 0.05, 0.10, 0.15), and the mole ratio of Li, Bi, Ho, Yb, and Ti is equal to x: 3.46: 0.04: 0.5: 3, where x denotes nominal Li doped content (CN) in Bi3.46Ho0.04Yb0.5Ti3O12: xLi. During the fabrication of Bi3.46Ho0.04Yb0.5Ti3O12: xLi phosphors, LiNO3 (99%, Macklin, Shanghai, China), Bi(NO3)3·5H2O (99%, SCRC, Shanghai, China), Ho(NO3)3·6H2O (99.99%, Rknerc, Shanghai, China), Yb(NO3)3·5H2O (99.99%, Rknerc, Shanghai, China) and Ti(OC4H9)4 (AR, Macklin, Shanghai, China) were used as the precursors of Li, Bi, Ho, Yb, and Ti ions, respectively. Ho, Yb, and Ti precursors were weighed according to stoichiometry of the formula of Bi3.46Ho0.04Yb0.5Ti3O12: xLi, and Bi and Li precursors exceeded 15% and 10% to supplement Bi and Li loss because both of them can partly volatilize during high-temperature treatment [20]. At first, the weighted Li, Bi, Ho, Yb precursors were put into a beaker, and then 15 mL acetic acid (AR, Macklin, Shanghai, China) was added rapidly, followed by heated under 55 °C and stirred for 15 min, and then cooled down to room temperature to obtain solution denoted as A liquid. 1.85 mL tetrabutyl titanate (AR, Macklin, Shanghai, China) was weighted and added into the other beaker containing 15 mL 2-methoxyethanol (AR, Macklin, Shanghai, China), and then stirred for 15 min to form B liquid. Subsequently, the B liquid was dropped into the A liquid gradually and stirred at 550 rpm for 2 h simultaneously under room temperature, and 0.06 Mol/L precursor solution with a golden color was obtained. The solution was dried in an oven at 80 °C until a solid gel was formed, and then sintered at 800 °C for 3 h in a muff furnace followed by cooling to room temperature under air atmosphere. The shape of the sintered product is fluffy, so they were ground in an agate mortar for 5 min to obtain the final BHYTO: xLi phosphor powders.
XRD (Rigaku D/MAX 2500V with a Cu Kα target, Rigaku, Tokyo, Japan) was performed to analyze phase structure of the samples, and the operated voltage and current are 40 KV and 100 mA, and the scanning range is from 10° to 60 ° with 5 °/min scanning speed, and the scanning step is 0.020. The lattice parameter and cell volume were calculated automatically through Jade 6.5 software based on the measured XRD data. Inductively coupled plasma emission spectrum (ICPMS Agilent 7700s, Agilent, Santa Clara, CA, USA) was used to assess Li+ practical content in the samples. SEM (Gemini Sigma 300/VP, Zeiss, Oberkochen, Germany) was used to analyze the morphology of the samples, operated at 5 kV with a standard beam current, and EDS to analyze elemental compositions of the samples. TEM (Titan G260−300, FEI Company, Hillsboro, OR, USA) was used to observe the morphological characteristics at high magnification. XPS (ESCALAB 250XI, Thermo Fisher Scientific, Waltham, MA, USA) was used to analyze the effects of Li+ doping on the structure and valance state of elements, and full spectrum scanning was performed in the range of 0 to 1000 eV with carbon peak correction at 284.6 eV before this analysis. Sample particle size was measured by Zeta potential (NanoBrook Omni, Brookhaven Instruments, Holtsville, NY, USA), and at the beginning of it, an appropriate amount of sample powders were placed in alcohol for ultrasound for 5 min to obtain a suspension with a concentration of about 0.6 mg/mL for measurement, and each sample was measured three times. An integrated fluorescence spectrometer (FluoroLog-3, Horiba, Kyoto, Japan) was used to measure the PLS and decay lifetime for the phosphors with a low noise 980 nm laser (MDL-III-980-2W, CNI Lasers, Changchun, China) as the pumping source. Note that all the samples had been dried at 120 °C for 2 h in a vacuum drying oven before the tests of the optical properties.

3. Results and Discussion

ICPMS measurement was performed to grasp whether Li+ was successfully doped into the fabricated BHYTO: xLi samples, and the results were shown in Table 1. The detected Li+ content (CD) in the final sintered products is less than that of the doped Li+ content (CP) in all the samples before sintering due to the volatilization of Li+. The detected Li+ content (CD) can be considered as Li+ practical content in the final compound of the phosphors ignoring measurement error. CD values are 1.70%, 4.88%, 9.92%, and 14.93% for the BHYTO: xLi phosphors with x equal to 0.02, 0.05, 0.10, and 0.15, respectively, and corresponding Li doping efficiencies (ηD) are 77.27%, 88.73%, 90.18%, and 90.48%. The values of CD and ηD increased with the increase in absolute mass for excessive Li+ dosage. Note that ηD was defined as the ratio of CD to doped Li+ content (CP). The results suggest that excessive dosage of 10% Li+ for the raw materials during the fabrication process is available. For the convenience of description, the nominal Li doped content was used to express Li+ content in all the BHYTO: xLi phosphors.
In order to obtain the structural information about phase, crystallinity, and crystal distortion of BHYTO: xLi phosphors, XRD was performed and the results were shown in Figure 1a. It can be seen that the phosphors consisted of dominant orthorhombic perovskite Bi4Ti3O12 phase and a small amount of pyrochlore Bi2Ti2O7 phases, and no other phase, such as Li2O or Li2TiO3, detected, suggesting that Li+ entered into the crystal lattice of bismuth titanates. It was reported that the radius of Bi3+, Ho3+, Yb3+, and Li+ was 0.103 nm, 0.090 nm, 0.087 nm, and 0.076 nm, respectively [21]. The diffraction peaks of pristine BHYTO without Li+ doping shifted toward larger angle in comparison with pure Bi4Ti3O12 phase (Card no. 35−0795), as shown in Figure 1b. Ho3+ and Yb3+ are inclined to substitute Bi3+ site in Bi4Ti3O12 [22] because of the same valence and close ion radius, and the substitution by smaller ion radius can result in crystal shrink. However, the diffraction peaks shifted towards smaller angle for BHYTO: 0.02Li sample compared to BHYTO samples, and then shifted towards larger angle gradually with further increase in Li+ content. The possible reason is that Li+ ions first entered into the interspaces of crystal lattice when its dosage was low and induced the expansion of the crystal cell, resulting in the shifts of diffraction peaks towards smaller angle. However, with the increase in Li+ dosage, the amounts of available interspaces in BHYTO crystal were reduced little by little, and Li+ began to occupy Bi3+ sites, causing volumetric shrinkage of the crystal cell and resulting in the shifts of diffraction peak towards a larger angle. Figure 1c shows the volume (VC) of crystal cell and grain sizes (DC) of crystal grains for the BHYTO: xLi phosphors with various Li+ content based on the XRD data of Figure 1a. The VC values first increased and then decreased while the DC increased monotonously with the increase in Li+ content in the BHYTO: xLi phosphors, and the DC values were calculated to be about 34.59 nm, 37.36 nm, 38.33 nm, 45.74 nm, and 48.17 nm for the BHYTO: xLi samples with x equal to 0, 0.02, 0.05, 0.1, and 0.15, respectively, according to famous Scherrer formula.
For an Aurivillius structured material, the lattice distortion and strain are usually expressed by the ratios of crystal parameters, that is, b/a and c/a, respectively, and the ratios increased with the increase in crystal distortion and strain increases [23]. Compared to Li+ undoped BHYTO, the degree of crystal distortion and strain were relieved significantly in Li+ doped BHYTO: xLi phosphors, because the ratio of b/a and c/a decreases gradually. However, the reduced full width at half maxima (FWHM), shown as Table 2, and increased grain sizes imply an enhanced crystallization in the Li+ doped samples. It was reported that Li2O can not only act as a flux to lower sintering temperature and promote the elemental diffusion so as to increase density and grain size of glass [24] and ceramics [25], but also act as catalyst to facilitate the synthesis of composite oxide [26], which could improve crystallization of products.
Figure 2 shows the SEM results for the BHYTO: xLi phosphors. It can be observed that all the BHYTO: xLi phosphors mainly consisted of micro-sized particles with irregular shape and most of the particles in weight had size in the range of 1 to 2 μm. There are some tiny particles on the surface of the micro-sized ones. EDS results show that the samples were composed of Bi, Yb, Ho, Ti, and O elements and no impurity element detected in the samples. The detected C element came from a graphite conductive adhesive tape used to adhere the sample powders during SEM measurement. Li+ was not detected by EDS due to its low atomic number. Figure 2g shows the content and average content of each element at 1 and 2 spot. It can be seen that the proportion of each element has little difference and is relatively consistent with the proportion of elements in Bi4Ti3O12. Figure 2h shows histogram of particle size for the samples, the particle size of all the samples changed little and was above 1 μm, which was consistent with the results in SEM.
Figure 3a shows TEM micrograph of BHYTO: 0.05Li sample with the optimal UC luminescence among all the BHYTO: xLi phosphors, and the micro-sized particles have a shape of small compact blocks. Figure 3b shows the selected area electron diffraction (SAED) pattern observed from c-axis direction, which presents a rectangle shape (in blue), and the length for the two intersecting edges of the rectangle is very close but not exactly the same, which is the structural feature of a typical orthorhombic crystal system. Figure 3c shows high-resolution transmission electron microscopy (HRTEM) image obtained by focus to a spot on the thin edge of a grain, where a fine and delicate crystal structure with regular atomic arrangement can be observed, and the distance between two neighboring parallel crystal planes in mutually perpendicular directions are 0.271 nm and 0.273 nm, corresponding to (200) and (020) crystal planes of Bi4Ti3O12, respectively [27]. Figure 3d shows (020) lattice fringe obtained from a filtering method through DM software (Digital Micrograph 3.7), where more regular structure of atomic array can be observed, and the vague areas in this image denoted as 1, 2, and 3 implies some defects of dislocations existed in the sample [28]. Figure 3e shows high-angle-annular-dark-field scanning transmission electron microscopy (HAADF-STEM) diagram and elemental distribution. The color of the object image is very bright, suggesting the phosphor contained some elements with large atomic number (i.e., Bi). The insert graphs in Figure 3 show the element compositions and distributions, and all the elements of Bi, Ho, Yb, Ti, O in the samples were detected except for Li elements due to its low atomic number, and the distributions of Bi, Ho, Ti, and O are uniform and dispersed more evenly than Yb element.
Figure 4a shows a full scan of XPS in the range of 0 to 1000 eV to analyze the chemical compositions and electron binding energy of BHYTO: 0.05 Li samples, and as a comparison, XPS of pristine BHYTO samples was also shown to illustrate Li+ doping effects. All the elements of Bi, Ti, O, Ho, Yb, and Li in the phosphors were detected though the peak of Li+ is very weak (see Figure A1 in Appendix A). Figure 4b shows high revolution XPS of Bi 4f, and there are two main peaks centered at 158.3 eV and 163.6 eV, very close to those of Bi 4f in Bi2O3 and BTO, corresponding to a pair of spin-orbit splitting energy of Bi 4f7/2 and Bi 4f5/2 [29]. Additionally, there is the other pair of smaller peaks with higher energy on the right, and both of the energy difference between these two pairs of peaks are equal to 5.3 eV, implying that they are both originated from electron transition of Bi 4f orbit. During high-temperature heat treatment process to produce Bi4Ti3O12 based materials, oxygen vacancies were easily formed on the surface of the samples, which created a crystal field environment around Bi3+ ions different from that of Bi3+ ions internal the body. In this work, BiS 4f and BiC 4f denote as Bi3+ ions near the surface and internal crystal lattice, respectively, and BiS 4f has a higher binding energy than BiC 4f. For BHYTO: 0.05Li phosphors, the peaks of BiS 4f shifted close to BiC 4f peaks and the area surrounded by BiS 4f curve and based line became smaller, which suggests Li+ doping had an effect on stabilizing oxygen in crystal lattice to make the environment around Bi3+ ions near the surface more similar to that in the body. As shown in Figure 4c, the peaks of 457.6 eV and 463.3 eV correspond to the characteristic binding energy of Ti 2p3/2 and Ti 2p1/2 [30], and the peak of Ti 2p1/2 overlaps with Bi 4d1/2 to form a wide energy peak. Note that nearly no change for the Ti 2p spectra indicates that Li+ did not substitute Ti4+ for the perovskite layer in BTO host. Figure 4d shows two symmetrical peaks at 529.1 eV and 530.9 eV, corresponding to the binding energy of O 1s [31]. They were denoted as lattice oxygen (OL) and absorbed oxygen (OA), respectively, and can be usually used as the probe for material oxygen vacancies. Compared to the XPS of BHYTO samples [22], O 1s peaks for BHYTO: 0.05Li sample have the same positions, but have a wider full width at half maximum (FWHM) and larger integrated curve area surrounded by XPS fitting curve and based line, suggesting that Li+ doping can stabilize oxygen in crystal lattice. This result is consistent with the previous analysis about Bi 4f spectra because of existing interaction between Bi and O elements. The XPS of Yb 4d and Ho 3p are shown in Figure 4e,f, where the values of FWHM and integrated curve area increased with Li+ doping for the same reason as Bi3+ 4f orbits, and Ho 3p peak shifted towards higher binding energy due to the charge repulsion effect of Li+ to the electrons in Ho 3p orbits. The reduced oxygen vacancies are consistent with the improvement of crystallinity for Li+ doped BHYTO phosphors. The results of XPS prove that the UC luminescence enhancement of BHYTO: xLi phosphors is not caused from increased oxygen vacancies.
Figure 5a shows the UC emission spectra of BHYTO: xLi phosphors under the excitation of 980 nm laser, there are three UC emission bands including a green band centered at 545 nm, a red one centered at 658 nm, and a near-infrared one at 756 nm for all the BHYTO: xLi phosphors. According to energy level analysis, these emission bands are assigned to the characteristic transitions of 5F4/5S2 → 5I8, 5F5 → 5I8, and 5F4/5S2 → 5I7 of Ho3+, respectively [32,33]. With the increase in Li+ content in BHYTO: xLi phosphors, the emission intensity increased gradually and reached an optimal value in BHYTO: 0.05 Li samples, which is about 2.2 times stronger than that of pristine BHYTO samples. However, the luminescence intensity decreased gradually with Li+ further doping though they are much stronger than that of BHYTO and BHYTO: 0.02Li samples. Figure 5b shows the decay time of carriers for the BHYTO: xLi phosphors monitored the dominant green emission (545 nm). Each curve in the graph represents the decay process with time for the carriers populated on Ho: 5F4/5S2 level. The decay data were well fitted by Equation (1) [34] with bi-exponent items,
I t = I 0 + A 1 e t τ 1 + A 2 e t τ 2
where, It denotes luminescence intensity at decay time t, and I0 denotes luminescence intensity at beginning decay time, Af and As are constants, and τf and τs represent two different decay lifetime for the bi-exponent items. Mean lifetime (τm) was expressed as Equation (2) [35].
τ m = t 0 I ( t ) I 0 dt
Based on the data in Figure 5b and Equation (2), the mean lifetime of Ho: 5F4/5S2 was calculated to be 55.28 μs, 65.99 μs, 57.51 μs, 46.22 μs and 45.25 μs for BHYTO: xLi samples with x equal to 0, 0.02, 0.05, 0.10, and 0.15, respectively. Compared to BHYTO: 0.02Li samples, the lifetime of BHYTO: xLi (x = 0.05, 0.10, 0.15) is shorter while the UC emission intensity is stronger.
As is well known, many factors might have effects on the emission efficiency of RE3+. In this article, the effects of charge compensation should be excluded because that charge compensation was used to apply in a charge imbalanced system, such as CaSrAl2SiO7: Ce3+ with the substitution of bivalent Sr2+ by trivalent Ce3+ [36], Ca3(PO4)2: Tb3+ with the substitution of bivalent Ca2+ by trivalent Tb3+ [17], and ZnO: Eu3+ with the substitution of bivalent Zn2+ by trivalent Eu3+ [37]. Codoping monovalent alkali element such as Li+, Na+, and K+ with the trivalent RE3+ can realize charge compensation. However, the situation is distinctly different. For the Bi3.46Ho0.04Yb0.5Ti3O12 samples without Li+ doping, it is a charge balanced system, and charge compensation is not necessary and the substitution of Bi3+ by Li+ can even lead to the imbalance of charge in the whole sample. So the luminescence enhancement by Li+ in this work seems not to be relevant with charge compensation. There is no obvious difference in particle size was observed for the samples with various Li+ contents. The results of SEM and Zeta potential suggest that the change of UC luminescence for BHYTO: xLi phosphors with different Li+ contents is not originated from particle size. The luminescence enhancement through Li+ doping in this study is also not caused by crystal distortion or increased strain. In order to further prove this viewpoint, Eu3+ doped BTO: xLi (BETO: xLi) samples were also fabricated in the same method as BHYTO: xLi phosphors. The PLS of Bi3.6Eu0.4Ti3O12: xLi (BETO: xLi, x = 0, 0.05, 0.1, 0.15) are shown in Figure A2a (in Appendix A) since Eu3+ is a famous luminescent probe to examine structural symmetry around a certain ion in lattice based on the ratio of emission intensity of 5D0 → 7F2 (electric-dipole-allowed transition) to 5D0 → 7F1 (magnetic-dipole-allowed one) of Eu3+ [16]. Eu3+ can be used as luminescent probe for BHYTO: xLi phosphors because it can substitute the same Bi3+ sites as Ho3+, Yb3+, and Li+ in BTO lattice through above XRD analysis. There are two strong red emission bands positioned at about 615 nm and 594 nm in PLS of BETO: xLi samples, corresponding to 5D0 → 7F2 and 5D0 → 7F1 transitions of Eu3+, respectively. As shown in Figure A2b (in Appendix A), the ratios decreased with the increase in Li+ doping content (0 ≤ x ≤ 0.15) in the BETO: xLi samples. This result reflected an increased structural symmetry and a decreased crystal distortion with the increase in Li+ content in the phosphors. Obviously, the luminescence enhancement was not originated from crystal distortion for BHYTO: xLi and BETO: xLi phosphors. For BHYTO: x Li phosphors, XRD results showed that the increase in Li+ doping content led to the gradual increase in grain size and promoted the improvement of crystallinity. XPS results showed that the oxygen vacancy defects gradually decrease and Li+ can act as a flux, which further confirmed that Li+ doping would improve the crystallinity of the sample. Furthermore, improved crystallinity of Li+ doped samples can increase oscillating strength for optical transitions, reduce quenching centers, such as density of grain boundary and oxygen vacancies [38], which is a main positive factor to improve emissions of RE phosphors. However, the UC luminescence is not only determined by crystallization since excessive Li+ doping (x ≥ 0.10) can make some RE ions squeezed out or deviated from their original sites in BHYTO lattice, leading to increased aggregation of RE ions, so, thus, decreasing the dispersibility of RE ions to produce local concentration quenching, so thus resulting in a weak degradation of UC emission intensity for BHYTO: xLi phosphors (x ≥ 0.10).
For a UC luminescent process, integral emission intensity (I) is usually proportional to the power (n) of pumping laser power (P), and the relationship formula is shown as Equation (3) [39],
I = P n
where index n denoted the number of absorbed photons in the UC process. Figure 6a,b show the dependence of UC intensities of green, red and near-infrared emissions on pumping power of 980 nm laser for BHYTO and BHYTO: 0.05Li samples, and the monitored emission wavelengths are 545 nm, 658 nm, and 756 nm, respectively. There appeared good linear fitting relationships between UC emission intensity and pumping power for all the emissions of each sample. The fitting index R2 values for each emission are all above 0.996 for BHYTO samples and above 0.992 for BHYTO: 0.05Li ones. The measured slope value is indicative of an upconversion process, which involves at least n photons, where n is the smallest integer greater than slope value (or equal to slope value if slope value is an integer) [40]. The slope values of all fitting lines are from 1.19 to 1.42, which lie in the range of 1 to 2, proving that the UC mechanism for BHYTO: xLi phosphors belong to a double-photon process for each of green, red and near-infrared emissions. The slope values of the fitting line deviate from the up limit of 2 and approaches close to the low limit value of 1. The deviation is caused from the competition between linear decay and UC processes for the depletion of the intermediate excited states. For a typical upconversion process mainly composed of three levels, if linear decay of the intermediate level is the dominant depletion, upconversion can be neglected, and, consequently, excited-state population densities (N2) in emission level has a relationship with excited-state population densities (N1) in intermediate level and pumping power (P): N2N12P2, corresponding to up limit of 2. In contrast, if upconversion is dominant, the linear decay term can be neglected, resulting in: N2N12P, corresponding to the lower limit of 1 [41]. The slope values are closer to the low limit, suggesting that upconversion is more obvious than decay for the depletion of the intermediate level. From another point of view, the low slop values reflect that BHYTO: xLi phosphors have relatively high upconversion efficiency. The phenomenon of low n value for double-photon upconversion process also occurs in Yb3+–Er3+doped BaTiO3 and Ho3+/ Er3+–Yb3+ co-doped NaLaMgWO6 [42,43].
The energy transfer process for the UC luminescence of BHYTO: xLi (x = 0, 0.02, 0.05, 0.10, 0.15) is shown in the Figure 7. Under 980 nm excitation, some Yb3+ ions absorbed the first photon energy and were pumped to exciting state from ground state (i.e., Yb: 2F7/2 + hv0 → Yb: 2F5/2), then transferred the energy to neighboring Ho3+ ions and excited them to intermediate 5I6 level (i.e., Yb: 2F5/2 + Ho: 5I8 → Yb: 2F7/2 + Ho: 5I6). Some Ho3+ ions populated in this level absorb the second photon energy transferred from Yb3+ and pumped to 5F4/5S2 levels (i.e., Yb: 2F5/2 + Ho: 5I6 → Yb: 2F7/2 + Ho: 5F4/5S2). When these Ho3+ ions in 5F4/5S2 transited to 5I7 and 5I8, a near-infrared emission centered at 756 nm and a green emission centered at 545 nm were produced (i.e., Ho: 5F4/5S2 → Ho: 5I7 + hv1, Ho: 5F4/5S2 → Ho: 5I8 + hv2), respectively. Some Ho3+ populated in 5I6 level decayed to the next 5I7 level through non-radiative relaxation, and then absorbed the second photon energy and pumped to 5F5 emission level (i.e., Yb: 2F5/2 + Ho: 5I7 → Yb: 2F7/2 + Ho: 5F5), finally producing a 658 nm red emission when they came back to ground level directly (i.e., Ho: 5F5 → Ho: 5I8 + hv3). The above emission process is a typical ET (energy transfer) process from Yb3+ to Ho3+. Which existed other energy transfer processes to produce the above emissions, such as GAT (energy transfer through absorption energy by ground state) [44] or EAT (excitation state absorption) [45], but ET process was mainly responsible for the energy transfer in Ho3+–Yb3+ co-doped phosphors because Yb3+ has much larger absorption section than Ho3+ for 980 nm exciting light. It is well agreement with the fact that the UC emission intensity is relatively weak for Ho3+ single-doped BTO phosphors [9].

4. Conclusions

In this study, a series of novel efficient Li+ doped BHYTO phosphors were fabricated successfully. The detected Li+ content (CD) is very close to the nominal doped one (CN) in the samples BHYTO: xLi samples with x ≥ 0.05 through ICPMS measurement. Li+ entered into the interspace of BHYTO crystal lattice when its dosage was low, and substitute Bi3+ sites with further increase in Li+ dosage. The crystallinity and grain sizes increase monotonously with the increase in Li+ content in BHYTO: xLi samples. Compared to BHYTO samples, the UC emission intensity of BHYTO: xLi increased obviously when x ≥ 0.05. UC emission mechanism of the BHYTO: xLi phosphors belong to a double-photon energy transfer process mainly through ET from Yb3+ to Ho3+ without Li+ direct participation. The causes of luminescence enhancement were discussed in details based on the results of XRD, SEM, TEM, EDS, XPS, and PLS measurements of Eu3+ doped BETO: xLi. The improved crystallization and reduced quenching centers such as oxygen vacancies promote light absorption from pumping source and increase oscillating strength for optical transitions, which have primary responsibility for the improved UC luminescence of BHYTO: xLi phosphors. It can be inferred that the method of luminescence enhancement in this study can probably be extended for the other RE phosphors with similar structure.

Author Contributions

Performing the experiments, F.R.; Data collection and analysis, F.R.; Writing initial draft, F.R.; Data collection, J.Z.; Performing the experiments, D.W.; Performing the experiments, X.W.; Data collection, X.W.; Conceptualization, F.G; Methodology, F.G.; Resources, F.G.; Supervision, F.G.; Validation, F.G.; Review and Revised manuscript, F.G.; Acquisition of the financial support for the project, F.G. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Programs for Natural Science Foundation of Guangxi (2019GXNSFAA185013), Science and Technology Major Project of Guangxi Province (AA18118030), and Guangxi Key Laboratory Development Foundation (GXYSSF1802).

Data Availability Statement

All data generated or analyzed during this study are included in this published article.

Acknowledgments

The authors thank financial support from the Programs for Natural Science Foundation of Guangxi (2019GXNSFAA185013), Science and Technology Major Project of Guangxi Province (AA18118030), and Guangxi Key Laboratory Development Foundation (GXYSSF1802).

Conflicts of Interest

The authors declare no competing interests.

Appendix A

Figure A1. High resolution XPS spectra of Li 1s.
Figure A1. High resolution XPS spectra of Li 1s.
Crystals 11 01220 g0a1
Figure A2. (a) The PLS and (b) the ratios of 615 nm/594 nm emission for Bi3.6Eu0.4Ti3O12: xLi (BETO: xLi, x = 0, 0.05, 0.1, 0.15).
Figure A2. (a) The PLS and (b) the ratios of 615 nm/594 nm emission for Bi3.6Eu0.4Ti3O12: xLi (BETO: xLi, x = 0, 0.05, 0.1, 0.15).
Crystals 11 01220 g0a2

References

  1. Meng, Z.; Zhang, S.; Wu, S. Power density dependent upconversion properties of NaYbF4: Er3+@NaYbF4: Tm3+@NaYF4 nanoparticles and their application in white–light emission LED. J. Lumin. 2020, 227, 117566. [Google Scholar] [CrossRef]
  2. Shin, J.; Kyhm, J.H.; Hong, A.R.; Song, J.D.; Lee, K.; Ko, H.; Jang, H.S. Multicolor tunable upconversion luminescence from sensitized seed–mediated grown LiGdF4: Yb, Tm–based core/triple–shell nanophosphors for transparent displays. Chem. Mater. 2018, 30, 8457–8464. [Google Scholar] [CrossRef]
  3. Lim, C.; Aleksandrovsky, A.; Atuchin, V.; Molokeev, M.; Oreshonkov, A. Microwave–employed sol–gel synthesis of scheelite–type microcrystalline AgGd(MoO4)2:Yb3+/Ho3+ upconversion yellow phosphors and their spectroscopic properties. Crystals 2020, 10, 1000. [Google Scholar]
  4. Tang, Z.; Han, W.; Huang, Z.; Qi, J.; Zhang, Y.; Yi, J.; Yuan, J.; Lu, T. Near–infrared luminescent properties of Ln: LaGdZr2O7 (Ln = Nd, Yb) transparent ceramics for solid–state laser applications. Ceram. Int. 2020, 46, 22270–22275. [Google Scholar] [CrossRef]
  5. Oppo, C.I.; Corpino, R.; Ricci, P.C.; Paul, M.C.; Das, S.; Pal, M.; Bhadra, S.K.; Yoo, S.; Kalita, M.P.; Boyland, A.J.; et al. Incorporation of Yb3+ ions in multicomponent phase–separated fibre glass preforms. Opt. Mater. 2011, 34, 660–664. [Google Scholar] [CrossRef]
  6. Badge, S.K.; Deshpande, A.V. Study of dielectric and ferroelectric properties of bismuth titanate (Bi4Ti3O12) ceramic prepared by sol–gel synthesis and solid state reaction method with varying sintering temperature. Solid. State. Ion. 2019, 334, 21–28. [Google Scholar] [CrossRef]
  7. Xie, X.; Wang, T.; Zhou, Z.; Cheng, G.; Liang, R.; Dong, X. Enhanced piezoelectric properties and temperature stability of Bi4Ti3O12–based Aurivillius ceramics via W./Nb substitution. J. Eur. Ceram. Soc. 2019, 39, 957–962. [Google Scholar] [CrossRef]
  8. Yang, Z.; Yan, L.; Yan, D.; Song, Z.; Zhou, D.; Yin, Z.; Qiu, J.; Chen, G. Color tunable upconversion emission in Yb, Er co–doped bismuth titanate inverse opal. J. Am. Ceram. Soc. 2011, 94, 2308–2310. [Google Scholar] [CrossRef]
  9. Gao, F.; Liu, H.F.; Ren, F.; Wang, K.T.; Li, X.S.; Wang, Y.B.; He, C.; Wei, Y.Z. Tunable structure and intensive upconversion photoluminescence for Ho3+–Yb3+ codoped bismuth titanate composite synthesized by sol–gel–combustion (SGC) method. Ceram. Int. 2019, 46, 3015–3022. [Google Scholar] [CrossRef]
  10. Gao, F.; Zhou, H.; Wu, G.H.; Qin, N.; Bao, D.H. Combination of strong blue up–conversion photoluminescence and greatly enhanced ferroelectric polarization in Tm3+–Yb3+–W6+– doped Bi4Ti3O12 thin films. J. Electrochem. Soc. 2011, 158, G128–G131. [Google Scholar] [CrossRef]
  11. Huang, H.; Liang, X.; Wang, Z.; Wang, P.; Zheng, Z.; Liu, Y.; Zhang, X.; Qin, X.; Dai, Y.; Huang, B. Bi20TiO32 nanoparticles doped with Yb3+ and Er3+ as UV, visible, and near–infrared responsive photocatalysts. ACS Appl. Nano Mater. 2019, 2, 5381–5388. [Google Scholar] [CrossRef]
  12. Bokolia, R.; Mondal, M.; Rai, V.K.; Sreenivas, K. Enhanced infrared–to–visible up–conversion emission and temperature sensitivity in (Er3+, Yb3+, and W6+) tri–doped Bi4Ti3O12 ferroelectric oxide. J. Appl. Phys. 2017, 121, 084101. [Google Scholar] [CrossRef]
  13. Xiang, G.; Liu, X.; Xia, Q.; Liu, X.; Xu, S.; Jiang, S.; Zhou, X.; Li, L.; Wu, D.; Ma, L.; et al. Design of a bi–functional NaScF4: Yb3+/Er3+ nanoparticles for deep–tissue bioimaging and optical thermometry through Mn2+ doping. Talanta 2021, 224, 121832. [Google Scholar] [CrossRef]
  14. Chung, J.H.; Ryu, J.H.; Eun, J.W.; Lee, J.H.; Lee, S.Y.; Heo, T.H.; Shim, K.B. High enhancement of green upconversion luminescence of Li+/Er3+/Yb3+ tri–doped CaMoO4. Mater. Chem. Phys. 2012, 134, 695–699. [Google Scholar] [CrossRef]
  15. Jia, Y.; Song, Y.; Bai, Y.; Wang, Y. Upconverted photoluminescence in Ho3+ and Yb3+ codoped Gd2O3 nanocrystals with and without Li+ ions. Luminescence 2011, 26, 259–263. [Google Scholar] [CrossRef] [PubMed]
  16. Yi, S.S.; Shim, K.S.; Yang, H.K.; Moon, B.K.; Choi, B.C.; Jeong, J.H.; Kim, J.H.; Bae, J.S. Improved cathodoluminescent characteristics of Y2O3: Eu3+ thin films by Li–doping. Appl. Phys. A 2007, 87, 667–671. [Google Scholar] [CrossRef]
  17. Jung, G.W.; Park, K. Effect of monovalent charge compensators on the photoluminescence properties of Ca3(PO4)2: Tb3+, A+ (A = Li, Na, K) phosphors. J. Mater. Sci. Technol. 2021, 82, 187–196. [Google Scholar] [CrossRef]
  18. Mao, C.; Yang, X.; Zhao, L. Simultaneous morphology control and upconversion fluorescence enhancement of NaYF4: Yb, Er crystals through alkali ions doping. Chem. Eng. J. 2013, 229, 429–435. [Google Scholar] [CrossRef]
  19. Jin, D.; Yang, J.; Miao, X.; Wang, L.; Guo, S.; Wang, N.; Wang, L. Highly enhanced photoluminescence of YBO3:Eu3+ micro–spheres by co–adding Li ion and alkaline−earth metal ions. Mater. Lett. 2012, 79, 225–228. [Google Scholar] [CrossRef]
  20. Gao, F.; Zhang, Q.; Ding, G.; Qin, N.; Bao, D. Strong upconversion photoluminescence and large ferroelectric polarization in Er3+−Yb3+−W6+ triply substituted bismuth titanate thin films prepared by chemical solution deposition. J. Am. Ceram. Soc. 2011, 94, 3867–3870. [Google Scholar] [CrossRef]
  21. Dong, M.; Li, X.; Chi, F.; Wei, X.; Yin, M.; Chen, Y. Trivalent Yb/Ho/Ce tri–doped core/shell NaYF4 nanoparticles for tunable upconversion luminescence from green to red. J. Rare. Earth 2017, 35, 629–636. [Google Scholar] [CrossRef]
  22. Bordj, S.; Satha, H.; Barros, A.; Zambon, D.; Jouart, J.P.; Diaf, M.; Mahiou, R. Spectroscopic characterization by up conversion of Ho3+/Yb3+ codoped CdF2 single crystal. Opt. Mater. 2021, 118, 111249. [Google Scholar] [CrossRef]
  23. Ramana, E.V.; Prasad, N.V.; Tobaldi, D.M.; Zavašnik, J.; Singh, M.K.; Hortigüela, M.J.; Seabra, M.P.; Prasad, G.; Valente, M.A. Effect of samarium and vanadium co–doping on structure, ferroelectric and photocatalytic properties of bismuth titanate. RSC. Adv. 2017, 7, 9680–9692. [Google Scholar] [CrossRef] [Green Version]
  24. Lu, B.X.; Chen, K.; Wang, W.L.; Jiang, B.B. Effects of Li2O and Na2O on the crystallization behavior of lime–alumina–based mold flux for casting high–Al steels. Metall. Mater. Trans. B 2014, 4, 1496–1509. [Google Scholar] [CrossRef]
  25. Oberžan, M.; Holc, J.; Buh, M.; Kuščer, D.; Lavrač, I.; Kosec, M. High–alumina porcelain with the addition of a Li2O–bearing fluxing agent. J. Eur. Ceram. Soc. 2009, 29, 2143–2152. [Google Scholar] [CrossRef]
  26. Hedden, D.B.; Torardi, C.C.; Zegarski, W. M’– RTaO4 Synthesis: Activation of the precursor oxides by the reaction flux. J. Solid. State. Chem. 1995, 118, 419–421. [Google Scholar] [CrossRef]
  27. Zhang, Y.; Chen, Z.; Lu, Z. A facile method for the preparation of colored Bi4Ti3O12–x nanosheets with enhanced visible–light photocatalytic hydrogen evolution activity. Nanomaterials 2018, 8, 261. [Google Scholar] [CrossRef] [Green Version]
  28. Chen, Y.; Yang, B.; Zhou, Y.; Wu, Y.; Zhu, H. Evaluation of pitting corrosion in duplex stainless steel Fe20Cr9Ni for nuclear power application. Acta. Mater. 2020, 197, 172–183. [Google Scholar] [CrossRef]
  29. Liang, J.; Zhu, G.; Liu, P.; Luo, X.; Tan, C.; Jin, L.; Zhou, J. Synthesis and characterization of Fe−doped β−Bi2O3 porous microspheres with enhanced visible light photocatalytic activity. Acta Mater. 2014, 72, 272–282. [Google Scholar] [CrossRef]
  30. Chang, M.J.; Cui, W.N.; Liu, J.; Wang, K.; Du, H.L.; Qiu, L.; Fan, S.M.; Luo, Z.M. Construction of novel TiO2/Bi4Ti3O12/MoS2 core/shell nanofibers for enhanced visible light photocatalysis. J. Mater. Sci. Technol. 2020, 36, 97–105. [Google Scholar] [CrossRef]
  31. Zhao, X.; Yang, H.; Cui, Z.; Wang, X.; Yi, Z. Growth process and CQDs−modified Bi4Ti3O12 square plates with enhanced photocatalytic performance. Micromachines 2019, 10, 66. [Google Scholar] [CrossRef] [Green Version]
  32. Ragin, T.; Baranowska, A.; Kochanowicz, M.; Zmojda, J.; Miluski, P.; Dorosz, D. Study of mid–infrared emission and structural properties of heavy metal oxide glass and optical fibre co–doped with Ho3+/Yb3+ Ions. Materials 2019, 12, 1238. [Google Scholar] [CrossRef] [Green Version]
  33. Pang, T.; Jian, R.H.; Xie, J.P.; Lu, W.H. Up–conversion luminescence and photo–thermal effect of KY3F10: Yb3+, Ho3+ nanocrystals. J. Phys. D Appl. Phys. 2018, 51, 355301. [Google Scholar] [CrossRef]
  34. Liu, F.; Deng, D.; Wu, M.; Chen, B.; Zhou, L.; Xu, S. Luminescent and thermometric properties of dual emitting Eu2+/Sm3+ co–doped Sr4La(PO4)3O phosphor based on energy transfer. J. Rare. Earth 2021, 39, 261–268. [Google Scholar] [CrossRef]
  35. Jiao, M.; Xu, Q.; Zhao, Y.; Wang, D.; Liu, L.; Yang, C. Photoluminescence properties and energy transfer of high thermal stable Na2GdPO4F2: RE (RE = Sm3+, Ce3+, Tb3+) phosphor for solid−state lighting. J. Lumin. 2020, 226, 117388. [Google Scholar] [CrossRef]
  36. Park, K.; Hakeem, D.A.; Pi, J.W.; Kim, S.W. Improvement of photoluminescence properties of Ce3+—doped CaSrAl2SiO7 phosphors by charge compensation with Li+ and Na+. Ceram. Int. 2018, 44, 1929–1934. [Google Scholar] [CrossRef]
  37. Park, K.; Hakeem, D.A.; Pi, J.W.; Jung, G.W. Emission enhancement of Eu3+–doped ZnO by adding charge compensators. J. Alloys Compd. 2019, 772, 1040–1051. [Google Scholar] [CrossRef]
  38. Guo, L.; Wang, Y.; Wang, Y.; Zhang, J.; Dong, P.; Zeng, W. Structure, enhancement and white luminescence of multifunctional Lu6O5F8: 20% Yb3+, 1% Er3+(Tm3+) nanoparticles via further doping with Li+ under different excitation sources. Nanoscale 2013, 5, 2491–2504. [Google Scholar] [CrossRef] [PubMed]
  39. Halubek, G.K.; Szymanski, D.; Tran, T.; Ferrari, M.; Lukowiak, A. Upconversion luminescence of silica–calcia nanoparticles co–doped with Tm3+ and Yb3+ Ions. Materials 2021, 14, 937. [Google Scholar] [CrossRef]
  40. Bai, Z.H.; Lin, H.; Imakita, K.; Montazami, R.; Fujii, M.; Hashemi, N. Synthesis of Er3+/Yb3+ codoped NaMnF3 nanocubes with single–band red upconversion luminescence. Rsc. Advances 2014, 4, 61891. [Google Scholar] [CrossRef] [Green Version]
  41. Pollnau, M.; Gamelin, D.R.; Lüthi, S.R.; Güdel, H.U.; Hehlen, M.P. Power dependence of upconversion luminescence in lanthanide and transition–metal–ion systems. Phys. Rev. B 2000, 61, 3337–3346. [Google Scholar] [CrossRef]
  42. Manoj, K.M.; Tristan, K.; Tanusree, M.; Christoph, B.; Kaushal., K.; Vineet, K.R.; Hans, H.; Ulrich, V. Incorporation of Zn2+ ions into BaTiO3: Er3+/Yb3+ nanophosphor: An effective way to enhance upconversion, defect luminescence and temperature sensing. Phys. Chem. Chem. Phys. 2015, 17, 20741. [Google Scholar]
  43. Zhang, J.; Jin, C. Electronic structure, upconversion luminescence and optical temperature sensing behavior of Yb3+–Er3+/Ho3+ doped NaLaMgWO6. J. Alloys Compd. 2018, 783, 84–94. [Google Scholar] [CrossRef]
  44. Zhang, T.; Yu, L.; Wang, J.; Wu, J. Microstructure and upconversion luminescence of Yb3+ and Ho3+ co−doped BST thick films. J. Mater. Sci. 2010, 45, 6819–6823. [Google Scholar] [CrossRef]
  45. Vishwakarma, P.K.; Rai, S.B.; Bahadur, A. Intense red and green emissions from Ho3+/Yb3+ co–doped sodium gadolinium molybdate nano–phosphor: Effect of calcination temperature and Intrinsic optical bistability. Mater. Res. Bull. 2021, 133, 111041. [Google Scholar] [CrossRef]
Figure 1. (a) XRD pattern, (b) an enlarged XRD graph in the range of 2θ = 29.8°–30.5°, and (c) the volume of crystal cell and grain sizes of BHYTO: xLi phosphors.
Figure 1. (a) XRD pattern, (b) an enlarged XRD graph in the range of 2θ = 29.8°–30.5°, and (c) the volume of crystal cell and grain sizes of BHYTO: xLi phosphors.
Crystals 11 01220 g001
Figure 2. SEM of the BHYTO: xLi samples with x values equal to (a) 0, (b) 0.05, (c) 0.10, (d) 0.15, respectively, and (e), (f) EDS of 1st and 2nd spots in Figure 2b, (g) the elemental content in the samples of the BHYTO: 0.05Li samples, and (h) histogram of particle size for the samples.
Figure 2. SEM of the BHYTO: xLi samples with x values equal to (a) 0, (b) 0.05, (c) 0.10, (d) 0.15, respectively, and (e), (f) EDS of 1st and 2nd spots in Figure 2b, (g) the elemental content in the samples of the BHYTO: 0.05Li samples, and (h) histogram of particle size for the samples.
Crystals 11 01220 g002
Figure 3. (a) TEM image, (b) SAED pattern, (c) HRTEM image, (d) fringes of (200) obtained by filtering, and (e) HAADF-STEM diagram and elemental distribution for BHYTO: 0.05Li samples.
Figure 3. (a) TEM image, (b) SAED pattern, (c) HRTEM image, (d) fringes of (200) obtained by filtering, and (e) HAADF-STEM diagram and elemental distribution for BHYTO: 0.05Li samples.
Crystals 11 01220 g003
Figure 4. (a) XPS survey scan spectrum of pristine BHYTO and BHYTO: 0.05Li samples, and high resolution XPS spectra of (b) Bi 4f, (c) Ti 2p and Bi 4d, (d) O 1s, (e) Yb 4d, and (f) Ho 3p.
Figure 4. (a) XPS survey scan spectrum of pristine BHYTO and BHYTO: 0.05Li samples, and high resolution XPS spectra of (b) Bi 4f, (c) Ti 2p and Bi 4d, (d) O 1s, (e) Yb 4d, and (f) Ho 3p.
Crystals 11 01220 g004
Figure 5. (a) UC PLS pumped by a 980 nm laser and the pumping power and its density were set to be 245 mW and 613 mW/cm2, respectively (b) decay time of carriers on 5F4/5S2 level of Ho3+ for BHYTO: xLi (x = 0, 0.02, 0.05, 0.10, 0.15) phosphors monitored at 545 nm emission.
Figure 5. (a) UC PLS pumped by a 980 nm laser and the pumping power and its density were set to be 245 mW and 613 mW/cm2, respectively (b) decay time of carriers on 5F4/5S2 level of Ho3+ for BHYTO: xLi (x = 0, 0.02, 0.05, 0.10, 0.15) phosphors monitored at 545 nm emission.
Crystals 11 01220 g005
Figure 6. Log-log diagram of the dependence of UC emission intensities for green, red and near-infrared emissions on pumping power (P) of 980 nm excitation for (a) BHYTO and (b) BHYTO: 0.05Li samples.
Figure 6. Log-log diagram of the dependence of UC emission intensities for green, red and near-infrared emissions on pumping power (P) of 980 nm excitation for (a) BHYTO and (b) BHYTO: 0.05Li samples.
Crystals 11 01220 g006
Figure 7. Schematic diagram of energy transfers during the UC process for BHYTO: xLi phosphors.
Figure 7. Schematic diagram of energy transfers during the UC process for BHYTO: xLi phosphors.
Crystals 11 01220 g007
Table 1. The results of ICPMS measurement for Li content in BHYTO: xLi samples (x = 0.02, 0.05, 0.10, and 0.15).
Table 1. The results of ICPMS measurement for Li content in BHYTO: xLi samples (x = 0.02, 0.05, 0.10, and 0.15).
Sample No.Sample NamesCN (mol%)CP (mol%)CD (mol%)ηD (%)
1BHYTO: 0.02Li22.21.7077.27
2BHYTO: 0.05Li55.54.8888.73
3BHYTO: 0.10Li10119.9290.18
4BHYTO: 0.15Li1516.514.9390.48
Notes: Nominal Li+ content (CN), doped Li+ content (CP) in the samples before sintering, detected Li+ content (CD) in the sintered products and Li+ doping efficiency (ηD) during the whole fabrication process.
Table 2. The crystal parameters and FWHM for the BHYTO: xLi phosphors.
Table 2. The crystal parameters and FWHM for the BHYTO: xLi phosphors.
Sample Namesa (Å)b (Å)c (Å)FWHM (°/rad)
BHYTO:0Li5.39305.422932.79410.263/0.00459
BHYTO:0.02Li5.40815.436732.81880.243/0.00424
BHYTO:0.05Li5.40115.429832.82780.237/0.00414
BHYTO:0.1Li5.40355.426632.80160.199/0.00347
BHYTO:0.15Li5.39935.425132.82190.189/0.00330
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Ren, F.; Zhou, J.; Wang, D.; Wang, X.; Gao, F. The Effects of Li+ Doping on Structure and Upconversion Luminescent Properties for Bi3.46Ho0.04Yb0.5Ti3O12: xLi Phosphors. Crystals 2021, 11, 1220. https://doi.org/10.3390/cryst11101220

AMA Style

Ren F, Zhou J, Wang D, Wang X, Gao F. The Effects of Li+ Doping on Structure and Upconversion Luminescent Properties for Bi3.46Ho0.04Yb0.5Ti3O12: xLi Phosphors. Crystals. 2021; 11(10):1220. https://doi.org/10.3390/cryst11101220

Chicago/Turabian Style

Ren, Feng, Jinlei Zhou, Dengpeng Wang, Xianran Wang, and Feng Gao. 2021. "The Effects of Li+ Doping on Structure and Upconversion Luminescent Properties for Bi3.46Ho0.04Yb0.5Ti3O12: xLi Phosphors" Crystals 11, no. 10: 1220. https://doi.org/10.3390/cryst11101220

APA Style

Ren, F., Zhou, J., Wang, D., Wang, X., & Gao, F. (2021). The Effects of Li+ Doping on Structure and Upconversion Luminescent Properties for Bi3.46Ho0.04Yb0.5Ti3O12: xLi Phosphors. Crystals, 11(10), 1220. https://doi.org/10.3390/cryst11101220

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.