1. Introduction
The single crystals of calcium orthovanadate (Ca
3(VO
4)
2) (CVO) are considered as a laser host material [
1]. It has been shown that the high optical damage threshold [
2] and nonlinear optical coefficients of CVO are comparable to those of potassium dihydrophosphate (KH
2PO
4) (KDP) [
3]; therefore, these crystals are potentially useful for frequency conversion of tunable laser sources. CVO possesses the trigonal space group R3c [
2], and, being acentric, demonstrates intense second harmonic generation. Recently, nominally pure CVO crystals, and those doped by Mn and rare earth elements (Tm, Ho), have become of special interest due to their potential application as a new active medium for 2 μm lasers [
4,
5,
6,
7].
Ferroelectricity in CVO single crystals was discovered by Glass et al. in 1978 [
2]. The ferroelectric phase transition temperature (
Tc = 1383 K) was determined by differential thermal analysis and dielectric studies. The spontaneous polarization value (
PS = 68 μC/cm
2) was calculated using an empirical dependence of
TC, because high conductivity prevented direct hysteresis measurements [
2]. It was claimed that the observations of electrical domains, pyroelectric behavior, and dielectric and thermal evidence of a phase transition “leave little doubt that this material is correctly classified as ferroelectric” [
2]. As-grown domain structure, revealed by etching, represented the shapeless domains up to millimeter size.
The domains at the surface of CVO plates, revealed by etching in a 0.5% boric acid solution, are usually imaged by optical microscopy [
2,
4,
5,
7]. Recently, it has been demonstrated that confocal Raman microscopy (CRM) [
8] and piezoelectric force microscopy (PFM) [
9] could be used for detail analysis of as-grown domain structure in CVO [
10]. Nevertheless, domain structure in the bulk of CVO single crystals is still unstudied.
In this paper, we present the results of an experimental study of as-grown domain structure in CVO by several methods of domain imaging: optical microscopy, PFM, and Cherenkov-type second harmonic generation (CSHG) [
11,
12]. The combination of imaging methods provided a unique opportunity for the comprehensive study of domain structure in the bulk, and allowed the revelation of the domain switching during cooling, under the action of the pyroelectric field.
2. Materials and Methods
The studied nominally pure CVO single crystals, and those doped with Mn ions (at 0.05% and 0.1%), were grown from the melt, in air, by the Czochralski method with pulling in [100] directions [
7]. The grown crystals were about 12 mm in diameter and up to 45 mm in length. Then, 0.6-mm-thick plates were cut perpendicular to the polar axis. A final surface treatment was done by mechanochemical polishing, using a PM5 machine (Logitech Ltd., Glasgow, UK) with 50 nm colloidal silica suspension (Allied High Tech Products, Inc., Compton, CA, USA). The polishing procedure revealed a shallow relief corresponding to the surface domain pattern, with a step height of about 100 nm, which was enough for obtaining optical contrast.
Both polar surfaces of the sample were studied by optical microscopy and PFM. Various imaging optical modes (transmitted and reflected light, phase contrast, and bright and dark fields) were realized by means of an optical microscope BX-61 (Olympus, Tokyo, Japan). PFM imaging was performed using an NTEGRA Aura scanning probe microscope (NT-MDT, Moscow, Russia) with silicon NSC-16 tips (MikroMasch, Sofia, Bulgaria), conductive platinum coating, and a typical curvature radius about 25 nm. AC modulation voltage with amplitude
Umod = 10 V and frequency
fmod = 20 kHz was applied between the tip and the silver-paste solid-bottom electrode. The obtained contrast of piezoelectric response proved that the optical images correspond to ferroelectric domains on the polar surface (
Figure 1).
Application of CSHG allowed us to obtain a set of 2D domain images at different depths, with spatial resolution of about 500 nm. This method was realized by means of a homemade setup based on an NTEGRA Spectra scanning probe microscope (NT-MDT SI, Moscow, Russia) with a Yb fiber laser (1064 nm, 40 mW). Treatment of the obtained data by the Blender 3D computer graphics software toolset allowed the construction of 3D domain images.
3. Results
3.1. Surface Domain Structure
As-grown domain structure, imaged on the polar surface of all the studied samples by optical microscopy, mostly consisted of rounded shapeless domains (
Figure 2). Bright-field transmitted-light optical microscopy allowed imaging of the domain walls on both polar surfaces simultaneously (
Figure 2a). The significant difference in the domain wall positions on the opposite polar surfaces proved the existence of charged domain walls in the bulk. Moreover, rounded isolated domains, with diameter below the sample thickness, reached, typically, only one surface, which indicated the absence of essential domain elongation in the polar direction. The typical domain size on the surface ranged from 50 μm to 1 mm.
3.2. Bulk Domain Structure
Complete information about domain shape in the bulk was obtained by CSHG. The 3D images of domains in CVO crystals were more complicated than those of domains formed during polarization reversal in lithium niobate (LN) and lithium tantalate (LT) crystals, which typically demonstrate a small tilt of the domain walls from the polar direction [
13,
14]. The domain wall images in the bulk of CVO crystals represent interferometric patterns (
Figure 3), which, according to Kampfe et al. [
15], correspond to abnormally tilted charged domain walls.
We used CSHG to image as-grown domains in the bulk of CVO crystals by recording XY scans at different focal depths with 13 μm steps (
Figure 3). According to [
15], every bright line in the images represents a cross-section of the domain wall at different depths. The axial displacement between cross sections was equal to 5.8 μm, for the used fundamental wavelength (
λ = 1064 nm). The depth of independent cross sections, recorded in a single XY scan, was defined by numerical aperture of the used objective. The local topology of the domain wall was calculated from the obtained XY scans. 3D reconstruction of the domain structure from
Figure 3 was obtained by deconvolution (
Figure 4) (see the rotated image in
Video S1 in Supplementary Materials).
Analysis of domain wall position in the bulk allowed us to observe that the domain wall tilt from the polar direction ranged from 11.2° to 71.4°, with an average value of about 35°.
It was demonstrated that as-grown domain structure in CVO crystals represented a 3D maze, with randomly oriented charged domain walls, strongly tilted from the polar direction. According to bulk imaging, isolated rounded domains rarely occurred. This fact indicates that optical images of rounded domains, observed on the polar surfaces, usually correspond to cross-sections of a large irregular domain maze.
The optically observed as-grown domain structure in both Mn-doped CVO crystals (
Figure 2b,c) looked similar to that of nominally pure ones (
Figure 2a). However, the essential difference between the shapes of isolated domains and domain walls of these crystals was revealed. In nominally pure CVO, all domains were rounded (
Figure 2a), whereas in 0.05% Mn-doped (
Figure 5a–c) and 0.1% Mn-doped CVO (
Figure 5d), single crystals sometimes showed triangular isolated domains and oriented flat fragments of domain walls, appearing together with rounded domains.
4. Discussion
The obtained results can be discussed in terms of kinetic approach [
16] to formation of as-grown domain structure during phase transition and subsequent cooling [
17]. The geometry of the domain structure, formed during slow cooling just below
TC, is determined by spatial distribution of the internal field, produced by bulk defects and composition inhomogeneities. The obtained absence of the quasi-regular layered domain structure justifies random spatial distribution of the defects, without pronounced growth striations [
18,
19,
20,
21,
22,
23]. Formation of charged domain walls is caused by low value of the depolarization field and high bulk conductivity, near
TC. The fast bulk screening of the depolarization field at high temperature stabilizes the formed domain pattern and provides its permanence during slow cooling [
17].
During fast cooling to the room temperature, the domain structure can change under the action of the pyroelectric field [
17,
24,
25], for implementation of the following relation:
where
Epyr.z(
T,
dT/
dt) is the polar component of the pyroelectric field, which depends on temperature and cooling rate, and
Eth(
T) is the temperature-dependent threshold field for domain switching.
It is important to point out that the shape of the isolated ferroelectric domains that arise during polarization reversal is defined by the crystal’s symmetry [
26]. A triangular or hexagonal shape in isolated domains is typical for uniaxial ferroelectric crystals of C
3 symmetry [
21,
27,
28]. The formation of flat domain walls is a result of determined step generation and kink motion along the wall [
26].
Thereby, it is possible to claim that, in nominally pure CVO crystals, the geometry of the as-grown domain structure, with rounded domains formed near TC, persists during subsequent cooling due to effective bulk screening of the depolarization field. The flat oriented fragments of domain walls and triangular domains in Mn-doped CVO appear during switching, under the action of the polar component of the pyroelectric field, above the threshold value. This fact represents the first observation of the domain switching in CVO crystals.
5. Conclusions
The domain structure formed after crystal growth in the paraelectric phase and cooling to room temperature, through the ferroelectric phase transition, was studied experimentally in nominally pure and Mn-doped calcium orthovanadate (CVO) crystals. Several methods were used for domain imaging: at the surface—optical microscopy and piezoelectric force microscopy, and in the bulk—Cherenkov-type second harmonic generation. Formation of an irregular 3D maze of rounded domains with charged walls, essentially tilted from the polar direction, was revealed in nominally pure and Mn-doped CVO crystals. The geometry of the domain structure formed during slow cooling, just below TC, is determined by spatial distribution of the internal field produced by bulk defects and composition inhomogeneities. The obtained absence of the quasi-regular layered domain structure justifies random spatial distribution of defects, without pronounced growth striations. The persistence of the domain structure with charged walls during cooling can be attributed to effective bulk screening of the depolarization field, and low value of the pyroelectric field. The rare formation of triangular domains and flat fragments of domain walls revealed in Mn-doped CVO was attributed to the action of the excess polar component of the pyroelectric field, above the threshold value for domain switching. This fact represents the first observation of domain switching in CVO crystals. Therefore, we plan to study domain switching in pure and Mn-doped CVO crystals under the action of the pyroelectric field, which arises during heating and cooling with controlled rates.
Author Contributions
Conceptualization, V.S. and E.S.; methodology, E.S.; software, E.L.; investigation, M.N., V.Y., and E.S.; resources, L.I.; writing—original draft preparation, E.S. and V.S.; writing—review and editing, V.S. and E.P.; visualization, M.N., V.Y. and E.S.; supervision, V.S.; project administration, V.S. All authors have read and agreed to the published version of the manuscript.
Funding
This research was funded by the Russian Foundation for Basic Research, grant number 20-02-00588-a, and the Ministry of Science and Higher Education of the Russian Federation, grant numbers 075-15-2021-677 and FEUZ-2020-0054.
Data Availability Statement
The data presented in this study are available on request from the corresponding author.
Acknowledgments
The equipment of the Ural Center for Shared Use “Modern nanotechnology” Ural Federal University (registration number 2968) was used.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Brixner, L.H.; Flournoy, P.A. Calcium orthovanadate Ca3(VO4)2—A new laser host crystal. J. Electrochem. Soc. 1965, 112, 303–308. [Google Scholar] [CrossRef]
- Glass, A.M.; Abrahams, S.C.; Ballman, A.A.; Loiacono, G. Calcium orthovanadate, Ca3(VO4)2—A new high-temperature ferroelectric. Ferroelectrics 1978, 17, 579–582. [Google Scholar] [CrossRef]
- Bechthold, P.S.; Liebertz, J.; Deserno, U. Linear and nonlinear optical properties of Ca3(VO4)2. Opt. Commun. 1978, 27, 393–398. [Google Scholar] [CrossRef]
- Ivleva, L.I.; Dunaeva, E.E.; Voronina, I.S.; Doroshenko, M.E.; Papashvili, A.G. Ca3(VO4)2:Tm3+—A new crystalline medium for 2-μm lasers. J. Cryst. Growth 2018, 501, 18–21. [Google Scholar] [CrossRef]
- Ivleva, L.I.; Dunaeva, E.E.; Voronina, I.S.; Doroshenko, M.E.; Papashvili, A.G.; Sulc, J.; Kratochvíl, J.; Jelinkova, H. Impact of Tm3+/Ho3+ co-doping on spectroscopic and laser properties of Ca3(VO4)2 single crystal. J. Cryst. Growth 2019, 513, 10–14. [Google Scholar] [CrossRef]
- Doroshenko, M.E.; Papashvili, A.G.; Voronina, I.S.; Ivleva, L.I.; Sulc, J.; Kratochvíl, J.; Jelinkova, H. Spectroscopic and laser properties of Tm3+ ions in Ca3(VO4)2 crystal. J. Lumin. 2019, 205, 482–486. [Google Scholar] [CrossRef]
- Voronina, I.S.; Voronov, V.V.; Dunaeva, E.E.; Iskhakova, L.D.; Papashvili, A.G.; Doroshenko, M.E.; Ivleva, L.I. Growth and properties of manganese doped Ca3(VO4)2 single crystals. J. Cryst. Growth 2021, 555, 125965. [Google Scholar] [CrossRef]
- Zelenovskiy, P.S.; Fontana, M.D.; Shur, V.Y.; Bourson, P.; Kuznetsov, D.K. Raman visualization of micro- and nanoscale domain structures in lithium niobate. Appl. Phys. A 2010, 99, 741–744. [Google Scholar] [CrossRef]
- Shur, V.Y.; Zelenovskiy, P.S. Micro- and nanodomain imaging in uniaxial ferroelectrics: Joint application of optical, confocal Raman and piezoelectric force microscopy. J. Appl. Phys. 2014, 116, 066802. [Google Scholar] [CrossRef]
- Shishkina, E.V.; Greshnyakov, E.D.; Zelenovskiy, P.S.; Yuzhakov, V.V.; Ivleva, L.I.; Shur, V.Y. Micro-Raman Domain Imaging in Calcium Orthovanadate Single Crystals. Ferroelectrics 2021, 576, 85–93. [Google Scholar] [CrossRef]
- Sheng, Y.; Best, A.; Butt, H.J.; Krolikowski, W.; Arie, A.; Koynov, K. Three-dimensional ferroelectric domain visualization by Čerenkov-type second harmonic generation. Opt. Express 2010, 18, 16539. [Google Scholar] [CrossRef] [PubMed]
- Kämpfe, T.; Reichenbach, P.; Schroder, M.; Haußmann, A.; Eng, L.M.; Woike, T.; Soergel, E. Optical three-dimensional profiling of charged domain walls in ferroelectrics by Cherenkov second-harmonic generation. Phys. Rev. B 2014, 89, 035314. [Google Scholar] [CrossRef]
- Esin, A.; Akhmatkhanov, A.; Shur, V. Tilt control of the charged domain walls in lithium niobate. Appl. Phys. Lett. 2019, 114, 092901. [Google Scholar] [CrossRef] [Green Version]
- Kirbus, B.; Godau, C.; Wehmeier, L.; Beccard, H.; Beyreuther, E.; Haußmann, A.; Eng, L.M. Real-time 3D imaging of nanoscale ferroelectric domain wall dynamics in lithium niobate single crystals under electric stimuli: Implications for domain-wall-based nanoelectronic devices. ACS Appl. Nano Mater. 2019, 2, 5787–5794. [Google Scholar] [CrossRef]
- Kämpfe, T.; Reichenbach, P.; Haußmann, A.; Woike, T.; Soergel, E.; Eng, L.M. Real-time three-dimensional profiling of ferroelectric domain walls. Appl. Phys. Lett. 2015, 107, 152905. [Google Scholar] [CrossRef]
- Shur, V.Y. Kinetics of ferroelectric domains: Application of general approach to LiNbO3 and LiTaO3. J. Mater. Sci. 2006, 41, 199–210. [Google Scholar] [CrossRef]
- Shur, V.Y.; Rumyantsev, E.L. Arising and evolution of the domain structure in ferroelectrics. J. Korean Phys. Soc. 1998, 32, S727–S732. [Google Scholar]
- Ming, N.-B.; Hong, J.-F.; Feng, D. The growth striations and ferroelectric domain structures in Czochralski-grown LiNbO3 single crystals. J. Mater. Sci. 1982, 17, 1663–1670. [Google Scholar] [CrossRef]
- Chen, J.; Zhou, Q.; Hong, J.F.; Wang, W.S.; Ming, N.B.; Feng, D.; Fang, C.G. Influence of growth striations on para-ferroelectric phase transitions: Mechanism of the formation of periodic laminar domains in LiNbO3 and LiTaO3. J. Appl. Phys. 1989, 66, 336–341. [Google Scholar] [CrossRef]
- Evlanova, N.F.; Naumova, I.I.; Chaplina, T.O.; Blokhin, S.A.; Lavrishchev, S.V. Periodically poled Y:LiNbO3 single crystal: Impurity distribution and domain wall location. J. Cryst. Growth 2001, 223, 156–160. [Google Scholar] [CrossRef]
- Shur, V.Y.; Gruverman, A.L.; Letuchev, V.V.; Rumyantsev, E.L.; Subbotin, A.L. Domain structure of lead germanate. Ferroelectrics 1989, 98, 29–49. [Google Scholar] [CrossRef]
- Blistanov, A.A.; Antipov, V.V.; Kugaenko, O.M.; Mikhailova, G.S. Effect of inhomogeneity on the formation of regular domain structures in LiNbO3 crystal. Crystallogr. Rep. 2002, 47, 111–116. [Google Scholar] [CrossRef]
- Bermúdez, V.; Caccavale, F.; Diéguez, E. Domain walls characterization of the opposite domain lithium niobate structures. J. Cryst. Growth 2000, 219, 413–418. [Google Scholar] [CrossRef]
- Shur, V.Y.; Kuznetsov, D.K.; Mingaliev, E.A.; Yakunina, E.M.; Lobov, A.I.; Ievlev, A.V. In situ investigation of formation of self-assembled nanodomain structure in lithium niobate after pulse laser irradiation. Appl. Phys. Lett. 2011, 99, 082901. [Google Scholar] [CrossRef] [Green Version]
- Shur, V.Y.; Kosobokov, M.S.; Makaev, A.V.; Kuznetsov, D.K.; Nebogatikov, M.S.; Chezganov, D.S.; Mingaliev, E.A. Dimensionality increase of ferroelectric domain shape by pulse laser irradiation. Acta Mater. 2021, 219, 117270. [Google Scholar] [CrossRef]
- Shur, V.Y.; Pelegova, E.V.; Kosobokov, M.S. Domain shapes in bulk uniaxial ferroelectrics. Ferroelectrics 2020, 569, 251–265. [Google Scholar] [CrossRef]
- Lobov, A.I.; Shur, V.Y.; Baturin, I.S.; Shishkin, E.I.; Kuznetsov, D.K.; Shur, A.G.; Dolbilov, M.A.; Gallo, K. Field induced evolution of regular and random 2D domain structures and shape of isolated domains in LiNbO3 and LiTaO3. Ferroelectrics 2006, 341, 109–116. [Google Scholar] [CrossRef] [Green Version]
- Shur, V.Y.; Nikolaeva, E.V.; Shishkin, E.I.; Chernykh, A.P.; Terabe, K.; Kitamura, K.; Ito, H.; Nakamura, K. Domain shape in congruent and stoichiometric lithium tantalate. Ferroelectrics 2002, 269, 195–200. [Google Scholar] [CrossRef]
| Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations. |
© 2021 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (https://creativecommons.org/licenses/by/4.0/).