Next Article in Journal
Thermal Stability, Dynamic Mechanical Analysis and Flammability Properties of Woven Kenaf/Polyester-Reinforced Polylactic Acid Hybrid Laminated Composites
Next Article in Special Issue
A Brief Review on Advanced Sandwich Structures with Customized Design Core and Composite Face Sheet
Previous Article in Journal
Comparison of Mechanical Properties of a Self-Adhesive Composite Cement and a Heated Composite Material
Previous Article in Special Issue
A Split-Wedge Anchorage for CFRP Cables: Numerical Model vs. Experimental Results
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Study on Bond-Slip Behavior between Seawater Sea-Sand Concrete and Carbon Fiber-Reinforced Polymer (CFRP) Bars with Different Surface Shapes

1
Department of Civil Engineering, Xiamen University, Daxue Road 182, Xiamen 361005, China
2
Mechanical Systems Engineering Laboratory, Empa, Swiss Federal Laboratories for Materials Science and Technology, Ueberlandstrasse 129, 8600 Duebendorf, Switzerland
*
Author to whom correspondence should be addressed.
Polymers 2022, 14(13), 2689; https://doi.org/10.3390/polym14132689
Submission received: 24 May 2022 / Revised: 23 June 2022 / Accepted: 27 June 2022 / Published: 30 June 2022

Abstract

:
The application of CFRP bar and seawater sea-sand concrete (SSSC) in construction can overcome the shortcomings in conventional reinforced concrete, such as corrosion induced by carbonation and chloride ingress. In this study, the bond-slip behavior between an SSSC cube and CFRP bar has been investigated, and different CFRP bar surface shapes have been considered. A total of 27 specimens (9 groups) were fabricated for a pull-out test, where three types of CFRP bar with different surface shapes were used: smooth regular bars, double-wrapped bars and ribbed bars. Bond strength, bond-slip curve, and failure mode have been presented and discussed. FE models have been constructed and validated by experimental results. The effect of concrete compressive strength and relative area of ribs on bond strength has been studied through numerical simulations. It is found that the bond strength increased with concrete compressive strength, and the ribbed bar had significantly higher bond strength than the smooth regular bar. Pull-out failure was observed when the cover-depth-to-bar-diameter ratio was no less than 4 and, otherwise, splitting failure occurred. In addition, a simple formula has been proposed to approximately evaluate the bond strength between an SSSC cube and CFRP bar and validated by experimental results, and analytical expressions for different bond-slip curves have also been developed.

1. Introduction

Seawater sea-sand concrete (SSSC) composed of sea-sand aggregate and seawater avoids material shortage in ocean construction and shows high economic value, attracting a lot of attention [1,2]. Li et al. [3] investigated the long-term performance of seawater sea sand and coral sand concrete. Saleh et al. [4] developed ultra-high-performance concrete by using seawater and sea sand. Qiao et al. [5] investigated the mechanical properties including elastic modulus, failure mode, strain–stress curve, etc. of SSSC subjected to variations of temperature. However, chloride ingress in SSSC causes and accelerates corrosion of steel rebar, leading to early deterioration of concrete and eventually to structural failure [6,7,8].
Therefore, in order to prevent the reinforced bars from being corroded by chloride ions in seawater and sea sand, the fiber-reinforced polymer (FRP) bar, which has great corrosion resistance and high tensile strength, is used instead of steel reinforcing bars to improve the concrete durability [9,10,11,12,13]. Mohamed et al. [14] investigated both durability and mechanical properties of concrete reinforced by basalt fiber-reinforced polymer (BFRP) bars and indicated that the durability was influenced by the resin type and bar size. Yu et al. [15] studied the effect of water and alkaline solution on durability of concrete reinforced by carbon–glass hybrid FRP bar. Dong et al. [16] conducted a life cycle assessment case study to show the environmental impact on seawater sea-sand concrete beam reinforced with glass fiber-reinforced polymer (GFRP) bars and CFRP bars.
So far, FRP bars have been widely used not only in marine engineering, but also in many other special constructions, due to the excellent mechanical properties and durability. The structural behavior of concrete reinforced by FRP bars is important for real applications, especially for flexural strength and shear strength. Jiang et al. [17] investigated the performance improvement of SSSC beams reinforced with FRP bars in serviceability limit state. Karayannis et al. [18] designed an experiment to investigate the behavior of slender concrete beams reinforced with CFRP bars including deflection, failure mode, and cracking pattern, etc. Ogrodowska et al. [19] presented the impact of nanomodification, hybridization and temperature on the shear strength of BFRP bars. Pang et al. [20] investigated the flexural behavior of two-span continuous CFRP bar-reinforced concrete beams. Roudsari et al. [21] proposed an optimization method to improve the structural performance of FRP bars-reinforced concrete columns by using nonlinear finite element (FE) model. Gu et al. [22] designed and conducted an experimental study to investigate the flexural properties of hybrid FRP bars-reinforced concrete beams. Guo et al. [23] developed a method based on accumulative damage model to predict the fatigue life of CFRP bar-reinforced concrete beams. Kim et al. [24] evaluated the structural performance of concrete structural component reinforced with FRP bars by different bars. Bakar et al. [25] reviewed the flexural strength of CFRP bar-reinforced concrete beams and indicated that both ACI 440.1R-15 and CSA S806-12 underestimate the ultimate flexural moment capacity of CFRP-reinforced concrete beams.
Besides structural behavior, bond performance between FRP bar and concrete is also important. Due to the difference in the chemical and mechanical properties between FRP and steel bars, the bond performance between FRP bar and concrete cannot be directly calculated using the traditional steel–concrete bond-slip model [26,27,28]. Yin et al. [29] investigated the bond performance between different types of FRP bars and all-coral aggregate seawater concrete by pull-out test, and showed that pull-out failure was mainly observed in specimens with smooth round bars and deformed CFRP bars and splitting failure was usually found in specimens with deformed BFRP and GFRP bars. In fact, the bond performance between FRP bars and concrete is affected by several factors such as material properties, and cover depth, etc. Many experimental and numerical studies have been conducted to investigate the factors influencing the bonding performance between FRP bars and concrete [30,31,32,33,34,35]. In particular, Caro et al. [36] analyzed the effect of FRP bar diameter, concrete strength, and bond length on the bonding performance between FRP bars epoxy-bonded into concrete. Veljkovic et al. [37] studied the influence of protective layer thickness on the bond performance between GFRP bars and concrete. They showed that the bond strength of ribbed GFRP bars was greater and the slip value was lower when the protective layer thickness was small, because the failure mode changed to splitting failure rather than pull-out failure. Jeong et al. [38] investigated the fatigue behavior of partially bonded CFRP bar-reinforced concrete beams subjected to cyclic load. Zhao et al. [39] carried out an experimental study to evaluate the bond behavior between CFRP bars, GFRP bars, steel strands and concrete, and pointed out the bond strength retention rate of GFRP bars was the highest, while that of steel strand was the lowest. Gong et al. [40] investigated the bond performance between CFRP bars and the cracked concrete interface by conducting experiments. Zhou et al. [41] investigated the bond performance between FRP bars and advanced sustainable concrete where seawater, sea sand, and recycled aggregates were used.
However, there is limited research on the bond behavior between CFRP bars and SSSC, due to the unique characteristics of CFRP bars, especially for different surface shapes of CFRP bars. Therefore, this paper conducted the pull-out tests on an SSSC cube with CFRP bar to investigate the bond performance and the main factors influencing the bonding performance, such as concrete compressive strength and relative area of ribs of a ribbed CFRP bar. In addition, refined FE models were constructed and validated by experimental results, based on which a simple formula was proposed to evaluate the bond strength approximately, and analytical expressions for different bond-slip curves were developed as well.

2. Experimental Program

The properties of the adopted SSSC cube and CFRP bar, and the test procedures and results, are presented in this section.

2.1. Material Properties

The seawater and sea sand used in this study were all produced naturally in Xiamen, China. The cement used in this study was ordinary Portland cement with compressive strength of 42.5 MPa after 28 days. The grain size distribution of sand and gravel aggregate can be seen in Figure 1. High performance polycarboxylate superplasticizer with a water reducing rate of 20% was used to ensure the proper workability of concrete. Class I fly ash was used as the admixture and the content was 20%. Three grades of concrete—C30, C40, and C50—were adopted in this study, and the details of concrete mixture can be seen in Table 1, where “W/C” ratio means the water-to-cement ratio.
High-adhesion carbon fiber prestressed bars were used as the CFRP bars, which had a diameter of 10 mm in this study. Three types of CFRP bars with different surface shapes, namely, smooth regular bars, double-wrapped bars, and ribbed bars, were selected. Figure 2 shows the three types of CFRP bars with different surface shapes, and Table 2 presents their elastic modulus and tensile strength, which were determined by tensile testing.

2.2. Specimens

Each specimen consisted of a CFRP bar, a PVC tube, a steel tube, and a concrete cube, as shown in Figure 3. The concrete cube for each specimen had the dimensions of 150 mm × 150 mm × 150 mm, followed by ACI 440.3R-12 [42], Chinese national code [43], and previous studies [34]. A steel tube was adhered to the loading end of CFRP bar to protect the bar during pull-out test, while the other end of the CFRP bar was freely exposed. The bond length between CFRP bar and concrete was 50 mm, and a 100 mm-long PVC tube was used to separate CFRP bar and concrete, because the ratio of embedded length to diameter of rebar should be 5 [42,43]. Once the specimens were cast, they were cured at standard conditions for 28 days.
In this study, the identification of specimen is determined as follows: the first letter indicates the CFRP bar type (S for smooth regular bar, D for double-wrapped bar, and R for ribbed bar), the first number indicates the grade of concrete, the second number indicates the ratio of cover depth to diameter of CFRP bar ( c / d ), and the last number donates the specimen number. For example, “S-50-7-3” designates the third specimen of the smooth regular CFRP bar-reinforced C50 SSSC cube with cover-depth-to-bar-diameter ratio of 7. A total of 27 specimens were cast in 9 groups based on orthogonal test design, which are listed in Table 3. For each group, three specimens were prepared to ensure data reliability.

2.3. Pull-Out Test

Figure 4 illustrates the experimental setup of pull-out test. The specimen was held by a frame consisting of two steel plate and four rods, the upper plate was connected to the test machine, and the lower plate had a hole to allow the CFRP bar to pass through. The relative slip between SSSC cube and CFRP bar were measured by LVDT. A universal testing machine was employed to apply the tensile load under displacement control at 0.5 mm/min.

2.4. Test Results

In the pull-out test, since the stress distribution is not uniform, which means that the shear stress along the axial direction ( τ x ) is not exactly a constant, the average bond stress along the embedded CFRP bar ( τ ) is therefore adopted:
τ = 0 l τ x d x l = P π d l
where P is the pull-out load measured by the universal testing machine, d is the diameter of CFRP bar, and l is the length of embedded CFRP bar. The relationship between the average bond stress and the unloaded CFRP bar end slip is used to analyze the bond behavior in this study. The test results have been summarized in Table 4, including the specimen ID, average bond strength, the peak slip related to the maximum load, and the failure mode (P = pull-out failure, S = splitting failure). In particular, the predicted bond strength by ACI 440.1R-06 [44] listed in Table 4 shows that the ACI code is not conservative for the bond strength between SSSC and CFRP bars with three different surface shapes, which indicates that this study is of significance.

2.4.1. Failure Mode

Two typical failure modes were observed during the pull-out tests: CFRP bar pull-out failure and concrete splitting failure.
For the CFRP bar pull-out failure, the surface of the concrete did not change significantly except that a small portion of the concrete near the bonding interface spalled off, and the CFRP bar was pulled out without damage, as shown in Figure 5a. Such failure mode occurred at the interface once the pull-out stress exceeded the shear bond strength between CFRP bar and concrete. Generally, when the ratio of cover depth to bar diameter ( c / d ) was no less than 4, the CFRP bar pull-out failure can be observed, since the surrounding concrete could still provide sufficient confinement to prevent splitting. This failure mode is usually preferred in actual application because it can provide an accurate evaluation of the bonding strength between CFRP bar and concrete.
For the concrete splitting failure, a large portion of the concrete spalled off, since the surrounding concrete can never provide adequate confinement before the pull-out stress exceeded the shear strength between CFRP bar and concrete, as shown in Figure 5b. There was a thin layer of concrete around the bar surface and the interface between CFRP bar and concrete was still undamaged, indicating that the bond strength was not attained. The radical stress due to the pull-out load initiated cracks in the radical direction from the interface, and the concrete confinement was not sufficient to prevent the crack propagation. This failure mode was only observed for smooth regular bar and double-wrapped bar when the ratio of cover depth to bar diameter was 2.

2.4.2. Bond-Slip Curves

As discussed above, there were two typical failure modes. Each failure mode has its own bond-slip relationship, which can be seen in Figure 6.
Figure 6a shows the bond-slip curve of smooth regular CFRP bar subject to bar pull-out failure (S-50-7-2, D-50-4-1, D-30-7-3). The bond stress increases gradually with the slip until the first peak. After reaching the maximum bond stress (bond strength), the interface between concrete and CFRP bar starts to damage, and the bond stress decreases slightly as the slip continues to increase. With the large increase in slip, the interface is damaged completely, and the bond stress comes from friction rather than bonding interface between concrete and bar. It should be noted that even if the interface was damaged completely in the test, the contact between concrete and bar was still close, and therefore, the bond stress only decreases from the peak value slightly in Figure 6a, which means that the friction can still provide resistance to slip between concrete and CFRP bar.
Figure 6b shows the bond-slip curve of ribbed CFRP bar subjected to bar pull-out failure (R-50-2-1, R-40-7-2, R-30-4-1). Different from the above bond-slip curve, the bond stress increases quickly with the slip at the initial stage, and it can reach the first peak when the slip is only 2 to 3 mm, which means that the bonding between ribbed bar and concrete is great, and the bond stress can achieve a high level with limited deformation of bar. With the increase in slip, the bond stress decreases slightly due to peeling off of some ribs and the corresponding damage of interface. However, the bond stress rises slightly again since the friction between concrete and damaged ribs increases with the increase in slip. Then, the same procedures repeat a few times, and therefore, the bond-slip curve fluctuates periodically.
Figure 6c represents the bond-slip curve of concrete splitting failure (D-50-4-3, D-40-2-1, S-30-2-2). Similarly to the initial stage of the bond-slip curve of CFRP bar pull-out failure, the bond tress rises gradually with the slip until maximum bond stress (bond strength). However, after the peak, the bond stress decreases suddenly because the radial cracks initiate and propagate quickly. Although the interface between concrete and bar is still undamaged, the bar and the nearly surrounding concrete separate from the concrete cube completely, and therefore, the bond-slip curve drops with a great negative gradient after the maximum value.

3. Numerical Analysis

FE models simulating the pull-out test of the three types of CFRP bars have been constructed by ABAQUS 2020 and validated by the experimental results. A parametric study has also been conducted to investigate the effect of different factors including concrete compressive strength, CFRP bar diameter, and relative size of rib on bond performance between an SSSC cube and CFRP bar.

3.1. FE Models

The FE models of three bars with different surface shapes are shown in Figure 7. The diameter for all three bars is 10 mm. The double-wrapped bar has wrapping spacing of 14 mm and the ribbed bar has rib spacing of 4 mm, rib height of 1 mm, and rib width of 2 mm.
The assembled FE model of an SSSC cube and CFRP bar is shown in Figure 8, where the general contact between concrete and CFRP bar was adopted in the FE models. In particular, “Hard Contact” was selected for normal behavior, “Friction” was selected for tangential behavior, and the friction coefficient was set to 0.5. “Finite sliding” was adopted as the sliding formulation to simulate the slip between the concrete and CFRP bar. A gap of 1 mm between concrete and bar was modeled to simulate the PVC pipe. All degrees of freedom of bottom surface of the concrete cube was restrained to simulate fixed boundary conditions. The load was applied to the end of CFRP bar by displacement control, coinciding with the pull-out test. C3D8R element (8-node cuboid element with reduced integration) was used for the concrete cube and regular CFRP bar, and C3D4 element (4-node tetrahedral element) was used for double-wrapped CFRP bar and ribbed CFRP bar. The size of mesh on the CFRP bar was around 1 mm, nearly one tenth of the CFRP bar diameter, to ensure the convergence. In fact, the convergence was checked and it showed that when the mesh size was less than one eighth of the CFRP bar diameter, the results converged. A cylindrical zone with diameter of 60 mm in center of the concrete cube was generated which had the same mesh size with the CFRP bar. The rest of the concrete cube had a mesh size of 4 mm to reduce the total mesh number. The total mesh number of FE models varied from 2 × 105 to 4 × 105.
The concrete damage plasticity (CDP) model was employed as the constitutive model of SSSC to simulate the smeared crack representation, and the detailed parameters can be seen in Table 5, where fb0/fc0 is the compression plastic strain ratio and K is the invariant stress ratio. It combines damage theory and plasticity theory, and it includes two main failure mechanisms, namely, tensile cracking and compression fractures. The material properties of CFRP bar were obtained from a static test, and they are listed in Table 5 as well. The stress–strain curve of CFRP bar measured in the static test was used as the material property of CFRP bar in the simulation, which can be achieved by keying in measured data in ABAQUS.

3.2. Verification of Proposed FE Models

The FE models have been verified by the experimental results. Figure 9 shows the comparison of bond-slip curves of S-50-7-2 and R-40-7-2, obtained by experimental test and numerical simulation. It should be noted that the surrounding matrix has great stress and strain during the pull-out of the CFRP bar, and therefore, a cylindrical zone of 60 mm diameter having fine meshes had been used in the FE model. The bond stress by ABAQUS in Figure 9 was calculated as the average stress along the CFRP bar in the numerical simulation. Generally, the simulation results match the experimental results well. For specimen S-50-7-2, the maximum bond stress by numerical simulation is quite accurate, although the bond stress increases slightly slower than that measured in the test during the bond stress raising stage. For the specimen R-40-7-2, the FE model can accurately calculate the maximum bond stress and also the following fluctuation in bond-slip curve for the ribbed bar. Other bond-slip curves obtained by numerical simulations agree well with those from the experimental pull-out test, and they are not shown herein for brevity.

3.3. Parametric Study

Two factors, concrete compressive strength and relative size of rib, have been considered in this study to investigate the effect on the bond strength by the validated FE models.

3.3.1. Concrete Compressive Strength

An FE model of the regular bar with a diameter of 10 mm, ratio of cover depth to bar diameter of 7, was used to investigate the effect of concrete compressive strength on bond strength. Concrete compressive strength was used in the simulation, with 11 different values from 20 MPa to 80 MPa. Figure 10a shows the bond-slip curves with concrete compressive strength of 20 MPa, 40 MPa, 60 MPa, and 80 MPa, respectively. Since the concrete cover depth is sufficient, the CFRP pull-out failure can be observed. Therefore, the bond-slip curves rise to the maximum bond stress and then drop gradually, which coincides with the experimental observation. The relationship between bond strength and concrete strength is shown in Figure 10b. Generally, the bond strength between the concrete and CFRP bar increases as the concrete strength rises, but it should be noted that there is a plateau from 30 MPa to 40 MPa, which means that when the concrete compressive strength increases from 30 MPa to 40 MPa, the bond strength is still about 7.3 MPa without obvious increase. Figure 10b also shows the relationship between slip displacement related to the maximum bond stress and concrete strength, and the former slightly changes in the narrow range from 2 mm to 3 mm, although the latter increases from 20 MPa to 80 MPa, indicating that the concrete compressive strength has negligible influence on the slip displacement related to the maximum bond stress.

3.3.2. Relative Size of Rib

To investigate the effect of relative size of rib on bond strength, the FE model of the ribbed bar with diameter of 10 mm, ratio of cover depth to bar diameter of 7, and concrete compressive strength of 50 MPa was adopted. The relative size of rib is defined as the ratio of rib area to the cross-sectional area of CFRP bar, and five values, 0.15, 0.18, 0.23, 0.3, and 0.45, have been considered. Figure 11a shows the bond-clip curves with relative size of rib from 0.15 to 0.45. When the relative size of rib is in the range of 0 to 0.18, the CFRP bar pull-out failure occurs, so the bond stress decreases gradually after the maximum bond stress; when the relative size of rib is above 0.2, the failure mode changes to concrete splitting, and the bond stress drops drastically. Figure 11b shows the relationship between bond strength/slip displacement and relative size of rib. It is observed that when the relative size increases from 0 to 0.15, the bond strength increases significantly from 6.8 MPa to 12.5 MPa, and the corresponding slip displacement decrease from 2.5 mm to 1.0 mm, because of the presence of ribs. When the relative size of rib increases to 0.23, the failure mode changes to concrete splitting, and therefore, the bond strength and the corresponding slip displacement drops accordingly.

4. Analytical Model

In this section, a simple approximate formula of bond strength has been developed based on the numerical parametric study and validated by the experimental results. In addition, the analytical bond-slip curves for different failure mode has also been proposed.

4.1. Bond Strength

It is observed from the numerical study how the three factors influence the bond strength between CFRP bar and SSSC, and therefore, a simple formula of bond strength ( τ u ) is proposed as
τ u = β r β A β c
where
β r = 1.66 c d 0.29
is the factor of cover depth to diameter ( c / d ) ratio and it is obtained by fitting the curve in Figure 10b by least squares method, and
β A = 1.24 , Concrete   spliting   failure 1.80 , CFRP   bar   pullout   failure
is the factor of relative size of rib, and
β c = 2.96 f c 0.258
is the factor of concrete compressive strength ( f c ), and it is also obtained by fitting the curve in Figure 9b by the least squares method.
Figure 12 shows the comparison of bond strength calculated by the proposed formula and measured in the pull-out test. It is observed the formula can predict the bond strength well and conservatively, regardless of the type of CFRP bars. Therefore, the proposed expression of bond strength is applicable for all these types of CFRP bars.

4.2. Bond-Slip Curves

The analytical expression of bond-slip curves for the two failure modes have been proposed herein. Figure 13 shows the three typical bond-slip curves observed in the pull-out test. Generally, there are two parts in the bond-slip curve: the rising part where the chemical adhesive force plays a major role, and the sliding part where the bonding force is mainly due to friction.
For the regular bar and double-wrapped bar, the Malvar model [45] and linear model have been used for the rising part and sliding part, respectively, regardless of failure mode:
τ τ m = F s s m + G 1 s / s m 2 1 + F 2 s s m + G s / s m 2 , 0 s s m 1 k s s m 1 , s > s m
where s is the slip and s m is the slip displacement corresponding to the maximum bond stress, while F , G , and k are unknown parameters to be determined by experimental results.
For the ribbed bar, after the short sliding part from s m to s w , there is a fluctuating part due to the presence of ribs. Therefore, BPE model [46] and linear model have been adopted for the rising part and sliding part, respectively, and a fluctuation function has been selected for the fluctuating part:
τ = s / s m a , 0 s s m ( τ w τ m )   s + τ m s w τ w s m s w s m , s m s s w τ w γ e φ ω s s w cos s s w 1 + ρ e φ ω s s w 1 , s > s w
where a , γ , φ , ω , and ρ are unknown parameters to be determined by experimental results.
Figure 14 shows the fitted bond-slip curves of S-30-2-4, D-30-7-4, and R-40-7-2 for illustration, and Table 6 lists the values of unknown parameters determined by the test results. It is observed that the fitted bond-slip curves and the test results have a great agreement, indicating that the proposed analytical expressions can depict the characteristics of these three typical bond-slip curves well.

5. Conclusions

In this study, the bond-slip behavior between an SSSC cube and CFRP bar with different surface shapes has been investigated. A total of 27 specimens (9 groups) were fabricated for the pull-out test, where three different CFRP bar surface shapes were used, namely, smooth regular bars, double-wrapped bars and ribbed bars. Accordingly, bond strength, bond-slip curve, and failure mode have been presented and discussed. FE models of specimens have also been constructed and validated by the experimental results. The effect of concrete compressive strength and relative area of ribs on bond strength has been studied through numerical simulations. In addition, a simple formula has been proposed to approximately evaluate the bond strength between SSSC cube and CFRP bar and validated by test results. The proposed formula is more accurate than the provisions in ACI because the latter is more conservative. Analytical expressions for different bond-slip curves have also been developed. The main findings and conclusions are listed as follows:
  • In the pull-out test, the bond strength was highly dependent on the concrete compressive strength and the surface type of CFRP bars. The bond strength was higher if the concrete compressive strength value was larger, and the ribbed bar had significantly higher bond strength than the regular bar, which were further validated in the numerical simulations. From the numerical simulations, it is further observed that the increasing rate of bond strength became slower with the increase in concrete compressive stress.
  • There were two failure modes observed during the pull-out test mainly depending on the ratio of cover depth to bar diameter—CFRP bar pull-out failure and concrete splitting failure. When the ratio of cover depth to bar diameter was no less than 4, the CFRP bar pull-out failure was observed, and otherwise, the concrete splitting failure occurred, because cracks initiated due to pull-out-load-induced radical stress, and the concrete confinement was not sufficient to prevent the crack propagation.
  • The bond-slip curves for different failure mode were different. Generally, the bond stress dropped significantly after the maximum value for the concrete splitting failure and it decreased gradually (regular bars) or fluctuated slowly (ribbed bars) after the maximum value for the CFRP bar pull-out failure.
  • The proposed simple formula based on the parametric study can approximately predict the bond strength, which is more accurate than those in ACI, and the analytical expressions can depict the bond-slip curves for different failure modes and different shapes of CFRP bar.

Author Contributions

Conceptualization, J.G. and G.P.T.; methodology, J.G.; investigation, P.X. and L.F.; writing—original draft preparation, P.X.; writing—review and editing, J.G.; supervision, J.G.; project administration, J.G. All authors have read and agreed to the published version of the manuscript.

Funding

Natural Science Foundation of China (U2005216), Science and Technology Research and Development Plan of China Railway Group Limited (2020-Key-11), Natural Science Foundation of Fujian (2020J01010).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

We are grateful to the following agencies for their supports in this study: Natural Science Foundation of China (U2005216), Science and Technology Research and Development Plan of China Railway Group Limited (2020-Key-11), Natural Science Foundation of Fujian (2020J01010).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zhao, Y.; Hu, X.; Shi, C.; Zhang, Z.; Zhu, D. A review on seawater sea-sand concrete: Mixture proportion, hydration, microstructure and properties. Constr. Build. Mater. 2021, 295, 123602. [Google Scholar] [CrossRef]
  2. Xiao, J.; Qiang, C.; Nanni, A.; Zhang, K. Use of sea-sand and seawater in concrete construction: Current status and future opportunities. Constr. Build. Mater. 2017, 155, 1101–1111. [Google Scholar] [CrossRef]
  3. Li, Y.T.; Zhou, L.; Zhang, Y.; Cui, J.W.; Shao, J. Study on Long-Term Performance of Concrete Based on Seawater, Sea Sand and Coral Sand. Adv. Mater. Res. 2013, 706–708, 512–515. [Google Scholar] [CrossRef]
  4. Saleh, S.; Zhao, X.-L.; Hamed, E. Development of a Sustainable Industrial Byproduct Based Seawater and Sea Sand Ultra-High Performance Concrete. Environ. Sci. Proc. 2021, 12, 20. [Google Scholar] [CrossRef]
  5. Qiao, S.; Xiong, Z.; Li, Y.; Ye, Z.; He, S.; Li, L.; Zeng, Y. Mechanical Properties of Seawater Sea-Sand Concrete Exposed to Daily Temperature Variations. Buildings 2022, 12, 517. [Google Scholar] [CrossRef]
  6. Dhondy, T.; Remennikov, A.; Sheikh, M.N. Properties and Application of Sea Sand in Sea Sand–Seawater Concrete. J. Mater. Civ. Eng. 2020, 32, 04020392. [Google Scholar] [CrossRef]
  7. Jiang, Z.; Li, S.; Fu, C.; Dong, Z.; Zhang, X.; Jin, N.; Xia, T. Macrocell Corrosion of Steel in Concrete under Carbonation, Internal Chloride Admixing and Accelerated Chloride Penetration Conditions. Materials 2021, 14, 7691. [Google Scholar] [CrossRef]
  8. Kiesse, T.S.; Bonnet, S.; Amiri, O.; Ventura, A. Analysis of corrosion risk due to chloride diffusion for concrete structures in marine environment. Mar. Struct. 2020, 73, 102804. [Google Scholar] [CrossRef]
  9. Khan, M.U.; Ahmad, S.; Al-Gahtani, H.J. Chloride-Induced Corrosion of Steel in Concrete: An Overview on Chloride Diffusion and Prediction of Corrosion Initiation Time. Int. J. Corros. 2017, 2017, 5819202. [Google Scholar] [CrossRef] [Green Version]
  10. Hu, X.; Xiao, J.; Zhang, K.; Zhang, Q. The state-of-the-art study on durability of FRP reinforced concrete with seawater and sea sand. J. Build. Eng. 2022, 51, 104294. [Google Scholar] [CrossRef]
  11. Bazli, M.; Zhao, X.-L.; Raman, R.S.; Bai, Y.; Al-Saadi, S. Bond performance between FRP tubes and seawater sea sand concrete after exposure to seawater condition. Constr. Build. Mater. 2020, 265, 120342. [Google Scholar] [CrossRef]
  12. Morales, C.N.; Claure, G.; Emparanza, A.R.; Nanni, A. Durability of GFRP reinforcing bars in seawater concrete. Constr. Build. Mater. 2021, 270, 121492. [Google Scholar] [CrossRef]
  13. Lu, Z.; Su, L.; Xian, G.; Lu, B.; Xie, J. Durability study of concrete-covered basalt fiber-reinforced polymer (BFRP) bars in marine environment. Compos. Struct. 2020, 234, 111650. [Google Scholar] [CrossRef]
  14. Mohamed, O.A.; Al Hawat, W.; Keshawarz, M. Durability and Mechanical Properties of Concrete Reinforced with Basalt Fiber-Reinforced Polymer (BFRP) Bars: Towards Sustainable Infrastructure. Polymers 2021, 13, 1402. [Google Scholar] [CrossRef]
  15. Yu, Y.; Pan, Y.; Zhou, R.; Miao, X. Effects of Water and Alkaline Solution on Durability of Carbon-Glass Hybrid Fiber Reinforced Polymer Bars. Polymers 2021, 13, 3844. [Google Scholar] [CrossRef]
  16. Dong, S.; Li, C.; Xian, G. Environmental Impacts of Glass- and Carbon-Fiber-Reinforced Polymer Bar-Reinforced Seawater and Sea Sand Concrete Beams Used in Marine Environments: An LCA Case Study. Polymers 2021, 13, 154. [Google Scholar] [CrossRef]
  17. Jiang, J.; Luo, J.; Yu, J.; Wang, Z. Performance Improvement of a Fiber-Reinforced Polymer Bar for a Reinforced Sea Sand and Seawater Concrete Beam in the Serviceability Limit State. Sensors 2019, 19, 654. [Google Scholar] [CrossRef] [Green Version]
  18. Karayannis, C.G.; Kosmidou, P.-M.K.; Chalioris, C.E. Reinforced Concrete Beams with Carbon-Fiber-Reinforced Polymer Bars—Experimental Study. Fibers 2018, 6, 99. [Google Scholar] [CrossRef] [Green Version]
  19. Ogrodowska, K.; Łuszcz, K.; Garbacz, A. Nanomodification, Hybridization and Temperature Impact on Shear Strength of Basalt Fiber-Reinforced Polymer Bars. Polymers 2021, 13, 2585. [Google Scholar] [CrossRef]
  20. Pang, M.; Shi, S.; Hu, H.; Lou, T. Flexural Behavior of Two-Span Continuous CFRP RC Beams. Materials 2021, 14, 6746. [Google Scholar] [CrossRef]
  21. Roudsari, S.S.; Ungureanu, L.M.; Soroushnia, S.; Abu-Lebdeh, T.; Petrescu, F.I.T. Optimization of Fiber-Reinforced Polymer Bars for Reinforced Concrete Column Using Nonlinear Finite Element Algorithms. Algorithms 2022, 15, 12. [Google Scholar] [CrossRef]
  22. Gu, W.; Liu, H.; Dong, Y. Experimental Study on the Flexural Properties of Concrete Beams Reinforced with Hybrid Steel/Fiber-Belt-Bars. Materials 2022, 15, 3505. [Google Scholar] [CrossRef] [PubMed]
  23. Guo, X.-Y.; Wang, Y.-L.; Huang, P.-Y.; Zheng, X.-H.; Yang, Y. Fatigue Life Prediction of Reinforced Concrete Beams Strengthened with CFRP: Study Based on an Accumulative Damage Model. Polymers 2019, 11, 130. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  24. Kim, T.-K.; Park, J.-S.; Kim, S.-H.; Jung, W.-T. Structural Behavior Evaluation of Reinforced Concrete Using the Fiber-Reinforced Polymer Strengthening Method. Polymers 2021, 13, 780. [Google Scholar] [CrossRef]
  25. Bakar, M.B.C.; Muhammad Rashid, R.S.; Amran, M.; Saleh Jaafar, M.; Vatin, N.I.; Fediuk, R. Flexural Strength of Concrete Beam Reinforced with CFRP Bars: A Review. Materials 2022, 15, 1144. [Google Scholar] [CrossRef]
  26. Stark, A.; Classen, M.; Hegger, J. Bond behaviour of CFRP tendons in UHPFRC. Eng. Struct. 2019, 178, 148–161. [Google Scholar] [CrossRef]
  27. Akbas, T.T.; Celik, O.C.; Yalcin, C.; Ilki, A. Monotonic and Cyclic Bond Behavior of Deformed CFRP Bars in High Strength Concrete. Polymers 2016, 8, 211. [Google Scholar] [CrossRef] [Green Version]
  28. Kalupahana, W.; Ibell, T.; Darby, A. Bond characteristics of near surface mounted CFRP bars. Constr. Build. Mater. 2013, 43, 58–68. [Google Scholar] [CrossRef]
  29. Yin, S.; Hu, C.; Liang, X. Bonding Properties of Different Kinds of FRP Bars and Steel Bars with All-Coral Aggregate Seawater Concrete. J. Mater. Civ. Eng. 2020, 32, 04020282. [Google Scholar] [CrossRef]
  30. Cao, R.; Zhang, B.; Wang, L.; Ding, J.; Chen, X. Utilizing alkali-activated materials as ordinary Portland cement replacement to study the bond performance of fiber-reinforced polymer bars in seawater sea-sand concrete. Adv. Struct. Eng. 2022, 25, 1103–1113. [Google Scholar] [CrossRef]
  31. Zeng, J.-J.; Liao, J.; Zhuge, Y.; Guo, Y.-C.; Zhou, J.-K.; Huang, Z.-H.; Zhang, L. Bond behavior between GFRP bars and seawater sea-sand fiber-reinforced ultra-high strength concrete. Eng. Struct. 2022, 254, 113787. [Google Scholar] [CrossRef]
  32. Su, X.; Yin, S.-P.; Zhao, Y.-D.; Hua, Y.-T. Experimental study on bond behavior between BFRP bars and seawater sea-sand concrete. J. Central South Univ. 2021, 28, 2193–2205. [Google Scholar] [CrossRef]
  33. Zhao, Y.; Zhang, Y.; Yu, P.; Xu, J. Bond behavior of BFRP bars in concrete under lateral pressure. Polym. Compos. 2021, 42, 6080–6093. [Google Scholar] [CrossRef]
  34. Nepomuceno, E.; Sena-Cruz, J.; Correia, L.; D’Antino, T. Review on the bond behavior and durability of FRP bars to concrete. Constr. Build. Mater. 2021, 287, 123042. [Google Scholar] [CrossRef]
  35. Rolland, A.; Argoul, P.; Benzarti, K.; Quiertant, M.; Chataigner, S.; Khadour, A. Analytical and numerical modeling of the bond behavior between FRP reinforcing bars and concrete. Constr. Build. Mater. 2020, 231, 117160. [Google Scholar] [CrossRef]
  36. Caro, M.; Jemaa, Y.; Dirar, S.; Quinn, A. Bond performance of deep embedment FRP bars epoxy-bonded into concrete. Eng. Struct. 2017, 147, 448–457. [Google Scholar] [CrossRef] [Green Version]
  37. Veljkovic, A.; Carvelli, V.; Haffke, M.M.; Pahn, M. Effect of Small Concrete Cover on the Fatigue Behavior of GFRP Bars and Concrete Bond. J. Compos. Constr. 2019, 23. [Google Scholar] [CrossRef]
  38. Jeong, Y.; Kim, W.; Gribniak, V.; Hui, D. Fatigue Behavior of Concrete Beams Prestressed with Partially Bonded CFRP Bars Subjected to Cyclic Loads. Materials 2019, 12, 3352. [Google Scholar] [CrossRef] [Green Version]
  39. Zhao, J.; Luo, X.; Wang, Z.; Feng, S.; Gong, X.; Shumuye, E. Experimental Study on Bond Performance of Carbon- and Glass-Fiber Reinforced Polymer (CFRP/GFRP) Bars and Steel Strands to Concrete. Materials 2021, 14, 1268. [Google Scholar] [CrossRef]
  40. Gong, Y.; Shan, Y.; Wu, Y.; Wang, L.; Liu, X.; Ding, F. Bond Properties of Carbon Fiber Reinforced Polymer and Corrosion-Cracked Reinforced Concrete Interface: Experimental Test and Nonlinear Degenerate Interface Law. Materials 2021, 14, 5333. [Google Scholar] [CrossRef]
  41. Zhou, Y.; Wu, G.; Li, L.; Guan, Z.; Guo, M.; Yang, L.; Li, Z. Experimental Investigations on Bond Behavior between FRP Bars and Advanced Sustainable Concrete. Polymers 2022, 14, 1132. [Google Scholar] [CrossRef]
  42. ACI Committee 440.3R-12; Guide Test Methods for Fiber Reinforced Polymers (FRPs) for Reinforcing or Strengthening Concrete Structures. American Concrete Institute: Farmington Hills, MI, USA, 2021.
  43. GB/T50152-2012; Standard for test method of concrete structures. China Academy of Building Science: Bejing, China, 2012.
  44. ACI440.1R-06; Guide for the Design and Construction of Structural Concrete Reinforced with FRP Bars. American Concrete Institute: Indianapolis, IN, USA, 2006.
  45. Malvar, L.J. Tensile and bond properties of GFRP reinforcing bars. ACI Mater. J. 1995, 92, 276–285. [Google Scholar]
  46. Cosenza, E.; Manfredi, G.; Realfonzo, R. Behavior and Modeling of Bond of FRP Rebars to Concrete. J. Compos. Constr. 1997, 1, 40–51. [Google Scholar] [CrossRef]
Figure 1. Grain size distribution of sand and gravel aggregate.
Figure 1. Grain size distribution of sand and gravel aggregate.
Polymers 14 02689 g001
Figure 2. CFRP bars with different surface shapes: (a) smooth regular bars; (b) double-wrapped bars; (c) ribbed bars.
Figure 2. CFRP bars with different surface shapes: (a) smooth regular bars; (b) double-wrapped bars; (c) ribbed bars.
Polymers 14 02689 g002
Figure 3. Pull-out specimen: (a) photograph; (b) illustration.
Figure 3. Pull-out specimen: (a) photograph; (b) illustration.
Polymers 14 02689 g003
Figure 4. Experimental setup of pull-out test: (a) photograph; (b) illustration.
Figure 4. Experimental setup of pull-out test: (a) photograph; (b) illustration.
Polymers 14 02689 g004
Figure 5. Different types of failure mode: (a) CFRP bar pull-out failure; (b) concrete splitting failure.
Figure 5. Different types of failure mode: (a) CFRP bar pull-out failure; (b) concrete splitting failure.
Polymers 14 02689 g005aPolymers 14 02689 g005b
Figure 6. Bond-slip curves of different failure mode (a) bar pull-out failure (smooth regular CFRP bar) (b) bar pull-out failure (double ribbed CFRP bar) (c) concrete splitting failure.
Figure 6. Bond-slip curves of different failure mode (a) bar pull-out failure (smooth regular CFRP bar) (b) bar pull-out failure (double ribbed CFRP bar) (c) concrete splitting failure.
Polymers 14 02689 g006aPolymers 14 02689 g006b
Figure 7. FE models of (a) regular bar. (b) double-wrapped bar, and (c) ribbed bar.
Figure 7. FE models of (a) regular bar. (b) double-wrapped bar, and (c) ribbed bar.
Polymers 14 02689 g007
Figure 8. Assembled FE model of CFRP bar and SSSC cube.
Figure 8. Assembled FE model of CFRP bar and SSSC cube.
Polymers 14 02689 g008
Figure 9. Comparison of bond-slip curves between experimental test and numerical simulation: (a) S-50-7-2; (b) R-40-7-2.
Figure 9. Comparison of bond-slip curves between experimental test and numerical simulation: (a) S-50-7-2; (b) R-40-7-2.
Polymers 14 02689 g009
Figure 10. Effect of concrete compressive strength on bond strength: (a) bond-clip curves; (b) relationship between bond strength/slip displacement and concrete strength.
Figure 10. Effect of concrete compressive strength on bond strength: (a) bond-clip curves; (b) relationship between bond strength/slip displacement and concrete strength.
Polymers 14 02689 g010
Figure 11. Effect of relative size of rib on bond strength (a) bond-clip curves (b) relationship between bond strength/slip displacement and relative size of rib.
Figure 11. Effect of relative size of rib on bond strength (a) bond-clip curves (b) relationship between bond strength/slip displacement and relative size of rib.
Polymers 14 02689 g011
Figure 12. Comparison of bond strength calculated by the proposed formula and measured in the pull-out test.
Figure 12. Comparison of bond strength calculated by the proposed formula and measured in the pull-out test.
Polymers 14 02689 g012
Figure 13. Typical bond-slip curves: (a) regular bar and double-wrapped bar subject to bar pull-out failure; (b) ribbed bar subject to bar pull-out failure; (c) regular bar and double-wrapped bar subject to concrete splitting failure.
Figure 13. Typical bond-slip curves: (a) regular bar and double-wrapped bar subject to bar pull-out failure; (b) ribbed bar subject to bar pull-out failure; (c) regular bar and double-wrapped bar subject to concrete splitting failure.
Polymers 14 02689 g013
Figure 14. Comparison of fitted bond-slip curves and test results.
Figure 14. Comparison of fitted bond-slip curves and test results.
Polymers 14 02689 g014
Table 1. Details of concrete mixture.
Table 1. Details of concrete mixture.
GradeW/C
Ratio
Seawater
(Kg/m3)
Coal Ash
(Kg/m3)
Cement
(Kg/m3)
Sand
Ratio
Sea Sand
(Kg/m3)
Gravel Aggregate
(Kg/m3)
Water
Reducer
(Kg/m3)
Total Mass
(Kg/m3)
Compressive Strength
/MPa
C300.52118470.7282.790.396756.261152.73.535245037.5
C400.42218487.27349.060.3666691156.34.363245049.0
C500.345184106.56426.240.344593.71134.25.328245058.9
Table 2. Mechanical properties of CFRP bars.
Table 2. Mechanical properties of CFRP bars.
Surface TypeElastic Modulus (GPa)Tensile Strength (MPa)
Smooth regular bars180.01862.3
Double-wrapped bars166.41670.5
Ribbed bars172.11634.0
Table 3. Details of specimens.
Table 3. Details of specimens.
GroupGrade of ConcreteSurface Typec/d
1C30S2
2C40D2
3C50R2
4C50D4
5C40S4
6C30R4
7C30D7
8C40R7
9C50S7
Table 4. Test results for pull-out specimens.
Table 4. Test results for pull-out specimens.
Specimen IDMeasured Bond Strength
MPa
ACI Bond Strength
MPa
Peak Slip (mm)Failure Mode
S-50-7-19.8214.784.52P
S-50-7-29.0214.783.13P
S-50-7-311.2114.783.95P
D-50-4-115.2714.278.24P
D-50-4-218.3114.2710.91P
D-50-4-316.1514.276.2S
R-50-2-112.5113.932.28P
R-50-2-21113.931.6P
R-50-2-313.7613.933.87P
S-40-4-110.413.0111.67P
S-40-4-214.8213.0118.1P
S-40-4-313.3713.0113.27P
D-40-2-114.0312.706.18S
D-40-2-21312.705.79S
D-40-2-313.7112.707.7S
R-40-7-116.8813.486.65P
R-40-7-212.7213.482.82P
R-40-7-316.7113.487.63P
S-30-2-18.2611.113.26S
S-30-2-29.0211.114.7S
S-30-2-39.6711.117.92P
D-30-7-110.8511.7912.83P
D-30-7-29.2111.7914.5P
D-30-7-313.4311.7911.59P
R-30-4-18.8211.381.98P
R-30-4-26.9511.381.12P
R-30-4-39.4211.381.96P
Table 5. Material properties of SSSC cube and CFRP bar.
Table 5. Material properties of SSSC cube and CFRP bar.
Density
(g/cm3)
Young’s Modulus (GPa)Compressive Strength
(MPa)
Tensile Strength
(MPa)
Poison RatioDilation AngleEccentricityfb0/fc0KViscosity Parameter
SSSC (C50)2.4230858.93.720.2300.11.160.6670.001
CFRP bar1.78170/17000.3/////
Table 6. Parameters adopted in Figure 13.
Table 6. Parameters adopted in Figure 13.
ParameterD-30-7-4S-30-2-4ParameterD-40-7-2
F 4.7884.363 a 0.72
G −3.083−2.682 γ 0.93
k −0.168−1.176 φ 0.07
ω 1.33
ρ −1.17
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Gao, J.; Xu, P.; Fan, L.; Terrasi, G.P. Study on Bond-Slip Behavior between Seawater Sea-Sand Concrete and Carbon Fiber-Reinforced Polymer (CFRP) Bars with Different Surface Shapes. Polymers 2022, 14, 2689. https://doi.org/10.3390/polym14132689

AMA Style

Gao J, Xu P, Fan L, Terrasi GP. Study on Bond-Slip Behavior between Seawater Sea-Sand Concrete and Carbon Fiber-Reinforced Polymer (CFRP) Bars with Different Surface Shapes. Polymers. 2022; 14(13):2689. https://doi.org/10.3390/polym14132689

Chicago/Turabian Style

Gao, Jing, Penghai Xu, Lingyun Fan, and Giovanni Pietro Terrasi. 2022. "Study on Bond-Slip Behavior between Seawater Sea-Sand Concrete and Carbon Fiber-Reinforced Polymer (CFRP) Bars with Different Surface Shapes" Polymers 14, no. 13: 2689. https://doi.org/10.3390/polym14132689

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.