Damage Resistance of Kevlar® Fabric, UHMWPE, PVB Multilayers Subjected to Concentrated Drop-Weight Impact

1
Chemistry Department, College of Science and Technology, Temple University, 1925 N 12th Street, Philadelphia, PA 19122, USA
2
Physics Department, College of Science and Technology, Temple University, 1925 N 12th Street, Philadelphia, PA 19122, USA
3
Mechanical Engineering Department, College of Engineering, Temple University, 1947 N 12th Street, Philadelphia, PA 19122, USA
*
Author to whom correspondence should be addressed.
Polymers 2024, 16(12), 1693; https://doi.org/10.3390/polym16121693
Submission received: 19 April 2024 / Revised: 22 May 2024 / Accepted: 28 May 2024 / Published: 14 June 2024
(This article belongs to the Special Issue Damping Mechanisms in Polymers and Polymer Composites)

Abstract

:
The impact resistance of layered polymer structures using polyvinyl butyral (PVB) in combination with Kevlar® fabric and ultra-high molecular weight polyethylene (UHMWPE) were fabricated and tested. Methods of wet impregnation and hot-press impregnation and consolidation of fabric with PVB and UHMWPE were used to manufacture multilayer constructs. All sandwich constructs were fixed to the surface of ballistic clay and subject to a free drop-weight test with a conical impactor having a small contact area. All tests were made at the same impact energy of 9.3 J and velocity of 2.85 m/s. The change in the resistance force was recorded using a piezoelectric force sensor at the time intervals of 40 μs. Using experimental force–time history, the change in the impactor’s velocity, the depth of impactor penetration, the energy transformation at various stages of impactor interaction with the sample, and other parameters were obtained. Three indicators were considered as the main criteria for the effectiveness of a sample’s resistance to impact: (1) minimum deformation, bulging, of the panel backside at the moment of impact, (2) minimum absorption of impact energy per areal density, and (3) minimal or, better yet, no destruction of structural integrity. Under the tested conditions, the rigid Kevlar–PVB–Kevlar sandwich at the frontside and relatively soft but flexible UHMWPE–Kevlar–UHMWPE layers in the middle helped to localize and absorb impact energy, while the backside Kevlar–PVB–Kevlar sandwich minimized local bulging providing the best overall performance. The front layer damage area was very shallow and less than two impactor tip diameters. The backside bulging was also less than in any other tested configurations.

Graphical Abstract

1. Introduction

Reducing the weight of protective panels of body armor and other defensive structures while maintaining their performance properties under repeated exposure to projectiles and impact from sharp objects is a priority research goal for their improvement. Currently, there are four main materials used in such panels including steel, ceramics, and polymers like polyethylene with ultrahigh molecular weight (UHMWPE), high density (HDPE), poly(p-phenylene terephthalamide) (PPTA), and combination of them. Each material has advantages and disadvantages. Historically, steel was the first reliable protective material. Its strengths are high toughness, stopping power, and high multi-hit capability. Its main disadvantage is high weight. In addition, steel deflects a large mass of shrapnel rather than absorbing the impact. Despite this, research efforts to improve the protective properties of steel and other metal alloys [1,2,3], including metamaterials [4] and metallic glasses [5], are underway. Ceramics have much higher stiffness and fracture strength and can decelerate a projectile rapidly. At the same time, these properties lead to material brittleness. Brittle behavior also means that structural cracks extend far from the point of direct impact. Even when the ceramic panel is not completely destroyed, its resistance to the next strike is significantly reduced [6]. In addition, ceramics are at least twice as heavy as polymers.
Among polymers, UHMWPE and PPTA are currently most often used as light armor protection, separately or together [7,8,9,10]. UHMWPE with a high level of crystallinity, despite a relatively low elastic modulus, has a very high fracture strain and, as a result, moderate toughness that allows to catch a bullet and localizes the effect of impact. However, the disadvantage of UHMWPE is its low melting point, which leads to its severe softening and deformation due to ballistic impacts. Its impact resistance allows it to provide protection only up to level II according to the American National Institute of Justice (NIJ) [11]. To obtain a higher level of protection, the thickness of the panel must be increased significantly, making the body armor uncomfortable to wear. At the same time, PPTA in the form of fiber and fabric, such as Kevlar® from DuPont, Wilmington, DE, USA [12], Twaron® from Teijin Aramid, Arnhem, The Netherland, and other aramids, is mainly used as a soft protective armor. It has a very high strength-to-weight ratio, high stiffness, significantly higher thermal stability than UHMWPE and, as a result, fairly high energy absorption [13]. The main disadvantages of the PPTA fibers are their low elasticity due to very high degree of crystallinity. Also, manufacturing of PPTA fibers is environmentally very unfriendly due to energy-intensive processes and use of large quantities of concentrated sulfuric acid. Minimizing its use would be very desirable. Moreover, PPTA fibers have a relatively short lifespan due to sensitivity to hydrolysis and ultraviolet (UV) irradiation [14,15,16]. These characteristics make it necessary to search for methods and coating materials which could alleviate such issues [16,17].
There are other polymers, fibers, and composites based on them that are analyzed for use in impact-resistive protection for warfare and also for the aerospace industry. Recently, several detailed reviews [18,19,20,21] have been devoted to the analysis of such materials and their hybridization in multilayer structures. However, it seems strange that the well-known thermoplastic polyvinyl butyral (PVB) has not been thoroughly analyzed for use in ballistic composites despite it successfully use as a bonding layer in laminated safety glass for automotive and architectural windows, preventing the crack propagation and the scattering of fragments in the event of an impact, and its good performance across wide strain rates and temperature ranges [22,23]. PVB has excellent adhesive properties, flows easily, and exhibits fast release and low solvent retention. This helps in the impregnation of yarns and fabrics, and the formation of thin film coatings [24]. Among other things, this polymer has good UV resistance and can extend the shelf life and use of PPTA by protecting it from external factors.
However, there are some examples of PVB research for use in light armor. The work conducted by Salman’s group [25,26] used 12 w% PVB-phenolic to coat Heracron® (Seoul, Republic of Korea) aramid fibers and thin films of PVB were used between woven kenaf (Hibiscus cannabinus L.) fibers to create a multilayer polymer composite. However, the goal of that research was focused on a potential replacement of aramid fibers with less expensive and environmentally friendly natural fibers. They studied the effect of stacking order and number of layers of kenaf and aramid on resistance to quasi-static [26] and ballistic impacts [25]. The results showed that, regardless of the order of layers, the best resistance was demonstrated by the composite without the use of kenaf. Several papers also reported the successful blending and chemical bonding of hydroxyl groups of PVB with phenolic and vinyl ester thermosets in combination with layers of aramid fabric reinforcements [27,28]. They reported that the absorption of impact energy by PVB-aramid composite is significantly higher than that of thermoset-aramid composites, but the former has a slightly greater deflection (trauma depth) due to its elasticity. The best results for both parameters, maximum energy absorption and minimum deflection, were shown by aramid composites made using a blend of PVB and thermosets. Another very recent work constructed a Kevlar® composite multilayer structure from the fabric layers pre-impregnated with 50/50 mixture of phenol formaldehyde and polyvinyl butyral resins [29]. They carried out torsion, delamination, compression, and ballistic tests, but focused on constructing and comparing mesoscale and continuum numerical models and comparing them with experimental results. PVB has also been used as a matrix in 3D woven jute yarn auxetic composites [30], combined with liquid crystal polyester and poly(ester-amide) matrix resins for Twaron™ ballistic aramid fabric [31], and again, blended into the composite matrix with an unsaturated polyester thermoset resin reinforced with woven glass fabric [32]. Thus, as far as we could find, PVB in ballistic composites was mainly used as an elastic additive to brittle thermosets to improve their impact resistance. Even so, there is very little systematic analysis.
In this work, we report for the first time the comparative analysis of all-polymer multilayer composites made with Kevlar®49 fabric, UHMWPE film, and PVB in different combinations. To understand and optimize ballistic properties, our study first tested the tensile behavior of PVB and UHMWPE films and then examined several different combinations of them with Kevlar fabric using the free drop-weight method [33]. The behavior of a material at relatively low impact velocities does not completely determine its behavior at higher velocities, so we are currently conducting ballistic tests and the results will be reported elsewhere.

2. Materials and Methods

2.1. Components and Chemicals

The multilayer structures fabricated and tested in this work consist of various combinations of components: the para-aramid plain fabric made from DuPont™ Kevlar® 49 (area density: 218 g/m2, thickness: 0.37 mm, plain weave, tow width and spacing 1.5 mm), UHMWPE film (molecular weight (3 − 5) × 106 g/mol, density: 0.94 g/cm3, 0.2 mm thick) both purchased from GoodFellow, UK, and polyvinyl butyral film of two different thicknesses 0.25 and 0.05 mm (Mowital® donated by Kuraray, Hattersheim, Germany [34]). Also, the following chemicals were used as received: polyvinyl butyral powder (molecular weight 67.09 g/mol, Sigma-Aldrich), acetone (ACS grade), and methanol (ultrapure, HPLC grade, Fisher Scientific).

2.2. Fabrication of Multilayers Structures

Kevlar® fabric, sheets of UHMWPE, and PVB films were cut in shape, 6″ × 6″, using the laser cutting machine (OMTech Laser, Anaheim, CA, USA, model SH-G350, 50 W CO2 laser). Some of the multilayer structures were made with pieces of UHMWPE film treated with oxygen plasma on each side for one minute in the Herrick Plasma Cleaner (PDC-32, Harrick Plasma Inc., Ithaca, NY, USA), using RF high-level and 0.8 Torr of oxygen pressure. Other structures were prepared with untreated UHMWPE films. Kevlar® fabric was cleaned in acetone, dipped in, and shaken for about 2 min, while PVB films were used as received.
In the manufacture of layered structures from their constituent parts, two main methods have been used (Scheme 1): wet impregnation of Kevlar® fabric with PVB-methanol solution and/or melt impregnation with PVB and/or UHMWPE films. In the first case, thermal consolidation with the remaining layers was carried out at the next step. In the second case, the impregnation and consolidation of all layers occurred simultaneously under the heat press. Wet impregnation was performed in the following way. PVB (10 g) powder (Sigma-Aldrich) was mixed and sonicated in 100 mL of methanol for 20 min to produce a completely transparent solution. A rectangular Kevlar® fabric was submerged in the methanol/PVB 10 wt% solution for three hours while being covered. The fabric was then removed from the methanol/PVB solution and left flat to dry overnight. Melt impregnation and consolidation of all layers were achieved using an air-operated automatic heat press with top and bottom heating plates and pressure regulator (DK20SP Digital Knight 16″ × 20″ Air Automatic Heat Press, GEO Knight & Co., Inc., Brockton, MA, USA). Heat pressing was carried out at 190 °C.

2.3. Tensile Measurements

Samples were laser cut in the form of standard dumbbell-shape following the ASTM D638 [35] requirements for plastic specimen thinner than 4 mm (type IV). The widest part of the sample was covered with and glued on both sides to a thick textured paper (cartridge paper) so that the flat serrated grips of the tensile machine would not pierce the polymer samples, ensuring there was no slippage and no deformation of this area during the test. Tinius Olsen model H5KT (Horsham, PA, USA) Universal Testing Machine (UTM) was used for unidirectional tensile measurements.

2.4. Drop-Weight Impact Device

Figure 1 shows the home-built drop-weight tower and its main components. There is a pulley at the top of the tower with the rope holding the electromagnet. This setup controls the height of the drop of and impactor assembly. The impactor assembly consists of a solenoid armature (90.4 g), additionally loaded mass, aluminum rod (20 mm diameter, 637.7 g), force sensor (26.6 g), and impactor (see Figure 1). The solenoid armature, machined from low carbon steel 1018, is the tail of the impactor assembly. The current through the solenoid (DC 24V, 10A, open frame 80N pull type electromagnet, JF-1683-24V) allows the impactor assembly to be held and released by computer control power supply. In this work, all measurements were carried out using a single impactor machined from O1 tool steel (Rockwell B95) having the dimensions indicated in Figure 1 and the mass 80.2 g.
The quartz piezoelectric ICP® force sensor (model 208C05, PCB Piezotronics, Depew, NY, USA, 22 kN range, 0.246 mV/N sensitivity, 1.05 N/mm stiffness, 36 kHz upper frequency limit, with a NIST traceable calibration) was mounted as an integrated link between aluminum rod and the impactor. This sensor is a few orders stiffer than samples under the test, thus the absorbed impact energy by the sensor is neglected. The shortest rise time of the sensor is approximately 6.9 μs, based on its nature frequency, so a recording frequency of 25 kHz and the corresponding time resolution 40 μs was chosen, which guarantees untruncated signal recording.
The specimen clamp assembly consists of two parallel aluminum plates with a 102 mm (4″) diameter hole in the center of each. The flat surface of both plates, support and top, where the test sample was placed and clamped, is 152 × 152 mm2 (6 × 6 in2). The applied compression by screws prevented slippage of the specimen in the clamp during the impact. After testing, each sample was visually inspected of the grip zone and impact zone. All measurements were carried out under conditions that the sample lies flat and gap-free on the clay (Sargent Art® Plastilina, non-hardening modeling clay (Sargent Art Inc., Hazleton, PA, USA)) surface. A stainless-steel jar (108 mm (4.25 in) in diameter and 140 mm (5.7 in) depth) was filled with clay and placed in a vacuum oven at approximately 60 °C for 48 h. The jar was taken out several times and the clay were compacted to ensure full filling and no air pockets. An extra amount of clay was added to the top surface of the jar after the clay container was bolted to the bottom of the base plate (see Figure 1) to ensure the clay surface was flush with the top surface of the base plate. After each measurement, the clay was leveled with a spatula, and its temperature was checked. All measurements were performed at 21.5 ± 0.5 °C laboratory temperature. Impact tests on clay without a sample were carried out on each measurement day at its beginning and end. Separately, a series of measurements of the effect of temperature on the impact resistance of the clay was conducted at the same velocities and impact energies as in the study of our materials. These results will be published separately.
The synchronized data acquisition system operates the following way. The rocker switch on the home-built power supply activates the relay and turns off the power to the solenoid, which initially holds the impactor at a fixed height. The same “release signal” is sent to the data acquisition system (MATLAB ver.9.1) to start collecting data points from the force sensor, and a secondary signal is sent to the Phantom camera to start recording the drop.
All measurements are recorded in the parameters of force–time, while the most important interpretation of the results is carried out in the parameters force–displacement. Therefore, the correct transformation of the measured data into important outcome parameters, such as stiffness, toughness, energy, etc., for the understanding, modeling, and development of new materials is necessary. This often requires the use of independent methods to obtain and verify the same final parameters.
The first parameter needed for quantitative analysis is the impactor velocity, v0, when it touches the specimen. The theoretical velocity was calculated based on the energy conservation principle. The potential energy must be equal to the kinetic energy:
m g h = 1 2 m v 2 ,   v 0 = 2 g h .
With the drop heights equal 422 ± 1 mm, and 9.802 m/s2 gravitational acceleration at the location of our lab, the impact velocity, v0, is 2.877 ± 0.003 m/s. These calculations do not take into account any types of friction, including air drag, that are always present in the system.
Since the sensor is a part of the impactor assembly and is very sensitive to acceleration, it was possible to determine the moment of separation of the impactor from the electromagnet based on its readings. Thus, by knowing the time of its fall until the moment of contact with the specimen and assuming zero initial velocity, one can calculate the impact velocity (v = g × t) from the force-sensor output. However, while the armature slides inside the solenoid, the force of friction plus the force of electromagnetic induction, due to the finite turn-off time of the solenoid, violates the law of free fall and acceleration is not equal to gravitational. The sensor signal recording is shown in the graph (Figure 2), where over the time interval (t1t2) the acceleration of the impactor increases. This makes it difficult to accurately determine impact velocity using this method. Estimates based on the time interval (t3t1) and (t3t2) give the impact velocity 2.98 m/s and 2.71 m/s, respectively. The average of these two values gives us 2.847, which agrees well with the above-calculated value of 2.877 m/s as an upper limit obtained from the principle of energy conservation. Considering that the mass of the impact assembly is 2297 g and the impact speed is 2.847 m/s, the impact energy is equal to 9.31 J.
Processing of drop-weight impact results was based on the methodology described in the ASTM standards [33,36]. Briefly, the direct measurements of the force versus time by the force sensor are converted to the force versus displacement data using the following transformations:
v t = v 0 1 m   0 t F e x p t   d t
s t = 0 t v t t d t
E x = i j F x d x
E t = 1 2 m v 0 2 v ( t ) 2 + m g · s t = E a + E e
where v0 is the impactor velocity at the touch moment, m is the mass of an impactor assembly, Fexp is force-sensor measurement output, and s(t) is the impactor displacement. The energy balance at any given time, E(t), or given position, E(x), and the energy transfer from the impactor to the specimen can be calculated either by the integration of the force–displacement curve, Equation (4), or by the energy balance, Equation (5), where Ea is the absorbed energy and Ee is the elastic energy. Here, i and j are any two points along the displacement curve. As a reference, all integration is conducted using the midpoint rule. The steps of such transformation are illustrated in Figure 3. In this way, all parameters of the impact resistance of the sample including the energy of absorption at different phases of impactor-specimen interaction can be calculated.

3. Results

3.1. Unidirectional Tensile Measurements

The construct of the studied multilayer composite structure is based on the components purchased from various sources listed above. It should be noted that the parameter values specified by the manufacturer are not always precise technical characteristics of the received materials. One example could be given about the characteristics of UHMWPE film from GoodFellow, where according to the product specifications, the tensile modulus is 0.2–1.2 GPa, tensile strength 20–40 MPa, and elongation at break 500%. As one can see, this covers a wide range of values, especially for tensile modulus, and cannot be used to analyze and understand the behavior of the multilayer composite structures. During the drop-weight impact tests, it turned out that the UHMWPE films also have a certain level of anisotropy with respect to the direction of the roll. To obtain precise parameters of the film, it was cut in two orthogonal directions relative to the twist of the roll. Tensile measurements of these samples were performed using different strain rates. Below are two figures representing the stress vs. strain behavior for the case when the samples were cut across the direction of the roll (Figure 4b) and along the direction of the roll twist (Figure 4c). Tensile measurements of PVM Mowital® 0.25 mm thick films were also performed at three strain rates (Figure 4e), the same as for UHMWPE. The measured parameters, and the secant modulus of elasticity, Es, calculated at 3% tensile strain and ultimate tensile strength (UTS) for UHMWPE and PVB films obtained at different loading rates and load directions, are presented in Table 3.

3.2. Drop-Weight Impact Test

Using a force–displacement history diagram (Figure 5), the stages of impact energy transfer to a composite specimen and how it behaves at each corresponding stage can be described. For comparison, this is illustrated using four samples representing three basic types of behavior shown in Figure 5a–c. In the first stage, the load curve moves from the touch point to the first bend relatively slowly. According to [36], this stage can be caused by the inertial effects in the striker and, in our case, is most likely the result of sample displacement with the low resistance due to its initial bulging, minor gaps, and irregularities remaining after it was placed on the clay baking surface and clamped. This is denominated as the preloading zone (PL). For stiff samples, this zone is significantly shorter and almost vanishes (e.g., Figure 5b). After this, the force–displacement diagram becomes steeper and approximately linear until the first crack or delamination appears (Fc, Figure 5b), or force approaches its peak or maximum value (Fm, Figure 5a). The slope of this curve is a measure of the system's elastic response and its relative stiffness (RS) [36]. In our case, when the sample lies on the clay baking surface, this parameter reflects both the order of transverse deformation and the magnitude of its longitudinal distribution. A detailed analysis of the experimental results will involve a three-dimensional reconstruction of the profile of the deformed sample and the response of the clay basin [37]. A quantitative comparison of this parameter for different samples requires considering the thickness of samples and the same experimental conditions.
In the next zone, features of the load–displacement behavior above Fc and around the peak load Fm reflect the type of deformation and the level of sample damage, if any. This can represent different failure modes—irreversible deformation without or with cracks, delamination, or complete sample fracture. In general, this is called the failure zone (FZ). None of the tested samples were pierced, but samples with a combination of Kevlar® and UHMWPE demonstrated irreversible deformation without any failure (Figure 5a), whereas, as a result of an impact on samples of Kevlar® with PVB, but without UHMWPE, (Figure 5b) the destruction is well recorded as sudden load drops and recovery. The post-test inspection revealed ruptures of the Kevlar® fibers and cracks in the PVB on the front side of the composite plate. In both extreme cases, a smooth funnel in Kevlar®–UHMWPE sample and a much smaller funnel but with breaks in Kevlar®–PVB sample, are visible clearly in optical photographs with a digital zoom (Figure 6a,b). The combination of Kevlar® fabric with PVB and UHMWPE as the back layer results in a visible reduction of fracture and sagging of the front surface and reduced bulging of the back surface (Figure 6d).
Noteworthy is the fact that after the peak load, Fm, there is a zone of rapid drop in force and continued penetration of the impactor (Figure 5). A likely explanation for this behavior could be a progressive sample damage beyond the maximum load [38] and the viscoelastic nature of these samples [39]. To fully understand its nature, a special set of measurements is required at various impact rates and energies.
The peak force value, Fm, corresponds to the maximum negative acceleration, or deceleration, of the penetrated impactor, whereas the maximum deformation corresponds to the moment when the penetrated impactor velocity reaches zero. After the impactor velocity changes from zero to a negative value, the impactor begins to move up together with sample, and the force continues to decrease. It corresponds to the elastic response of the target (ER) when the sample partially restores its initial thickness and position to the value of residual deformation (Rd). The measured force goes to zero at the moment when impactor separates from the sample surface. It now measures only a small negative value corresponding to the inertia of the deceleration until the striker reaches the highest rebound point. After that, it again begins to move down for a second strike. The maximum value of the released elastic energy in our measurements was not more than 11%. Therefore, the energy of the second impact is insignificant, and we do not take into account that this can cause additional deformation and damage. Also, any deformation of the steel impactor assembly is neglected since the stiffness of its components is several orders of magnitude higher, and the deformation of the sensor is negligible.
In Figure 5, the ER phase displays the release of the elastic component of the initial impact energy. As one can see, the ER of the sample with UHMWPE (Figure 5a) is more than twice that of the sample with PVB only (Figure 5b). Figure 7a shows the energy–time histories of behavior for three samples as in Figure 5 and for a thinner sample PE3K2 for contrast. In Figure 7b, the maximum deformation and the instant elastic recovery for these samples are shown for comparison. It should be noted that due to the viscoelastic nature of the composite panels, the final recovery of deformation is much greater than the immediate recovery recorded during each test. However, in this work, we do not have reliable qualitative measurements of the slow recovery process and one can only approximately measure the final state of its deformation after tens of minutes. So, for K5PE4, the final deformation is approximately 3.4 mm, and for K5PVB2PE2 it is about 2.5 mm, which is around 4.8 mm less than what was measured at the time of the test in both cases.
All the main results of the experimental data and their numerical analysis are given in Table 4. Also presented here are the maximum stresses arising on the sample surface at the peak impact force, considering the impactor flat tip with a diameter of 1.17 mm (Figure 1h) and a corresponding contact area of 1.07 mm2.

4. Discussion

When comparing the behavior of different multilayer composite structures (Figure 5), the first thing that becomes evident is the significantly lower peak load, Fm, for sample K5PVB3 (Figure 5b) and the accompanying wide zone and weak resistance to destruction. This is confirmed by photographs of the front and back sides (Figure 6b). On the frontside, one can see all possible damage—plastic deformation and cracking, fiber-matrix debonding, fiber fracture, and tow splitting. The backside is also deformed significantly. Tows are dislodged and some fibers are torn. This also means that the PVB layers are broken into pieces and fabrics are delaminated from polymer layers. This sample consists of five layers of Kevlar® fabric, three of which are impregnated with PVB polymer, and then all five are consolidated at the pressure and temperature of 190 °C.
The completely different force–displacement dependence is for sample K5PE4 (Figure 5a), consisting of five layers of Kevlar® fabric and four layers of UHMWPE films consolidated under hot pressing at 190 °C. In this case, no polymer cracking and fiber fracture is observed at the frontside (Figure 6a). At the same time, there is a large deformation of the backside (button image of Figure 6a). This deformation is not localized, and it is distributed over a significant distance from the point of impact. For this reason, it is difficult to see it in a photograph, and two white lines are added to help guide the viewer’s eye. In addition, a large elastic component leads to a significant transfer of momentum to a protected body, which can have a negative effect too.
The difference in behaviors of K5PE4 and K5PVB3 samples can be explained by the inherent difference in the tensile properties of UHMWPE and PVB (Figure 4). The PVB is stiffer and harder but has much less fracture strain than UHMWPE. Thus, at relatively low strain rate, their behavior is significantly different. It is known that polyethylene experiences a strain hardening at a higher loading rate [40,41], and PVB is a viscoelastic polymer with a strong temperature and load-rate dependence [22,42] too. Experiments to compare these results with ballistic measurements of the same structures are in progress and will be reported elsewhere.
By combining these two extreme cases, a set of layered samples from the Kevlar® fabric and both UHMWPE and PVB were created. The use of UHMWPE layers at the back in sample K4PVB1PE2 resulted in an increase in peak load and a decrease in its maximum deformation (Figure 5d, red dots). However, at the same time, the brittleness of the front layer was preserved, although the damage zone FZ decreased (Figure 6c). In the next set of samples, a layered structure K5PVB2PE2 was created where two layers of UHMWPE were embedded in the middle of the sandwich. This combination gives the best results in all parameters (see Table 4). Upon a very detailed examination, one can still notice two small resets in the load resistance, marked in Figure 5c as Fc1 and Fc2, although these destructions of the front layer are local and insignificant. Such localized failure only affects an area of less than two impactor tip diameters or less than two tows of yarn. There is no evidence of fibers being pulled out beyond this area. The backside deformation in the case of K5PVB2PE2 looks very similar to K5PE4, but, in fact, its value is much less (see Table 4). Here, it must be emphasized once again that the measured residual deformation during the test is not final, primarily due to the significant viscoelasticity of UHMWPE. For this reason, after a few minutes, the permanent deformation is significantly less than at the moment of impact, as was reported here earlier. However, for the object that needs to be protected, the only important parameters are the maximum penetration depth of the impactor and the impactor energy that the armor is capable of absorbing.
By analyzing the transfer of energy from the impactor to the panel as a function of time (Figure 7a) and as a function of displacement (Figure 7b) during deformation and ultimately possible penetration of the impactor into the sample, the following conclusions can be drawn. At the initial stage, in terms of time and displacement, K5PVB3 absorbs impact energy faster than other materials (Figure 7a green curve), which indicates it has higher stiffness, compared to others. As expected, PE3K2 has the lowest stiffness (Figure 7a, b blue curve) and relatively small elastic component, Ee, which indicates irreversible damage and significant plastic deformation at the applied impact energy. K5PE4 (brown curve) absorbs the most elastic energy and, accordingly, demonstrates maximum elastic deformation, which is then returned to the impactor for its rebound. Due to this, its residual deformation is relatively small and there is virtually no fabric destruction, but the main disadvantage of this structure is significant deflection and bulging upon impact (Table 4). The second most rigid structure, also as anticipated, is K5PVB2PE2 (Figure 7a,b red curves). At the same time, this structure accumulates more elastic energy than other structures except K5PE4. If we compare the stiffness and energy absorption behavior of K5PVB2PE2 and K4PVB1PE2 (it is not shown in Figure 7), the latter, which has one layer less of Kevlar® and one layer less of PVB is slightly weaker and less elastic. Here, it is necessary to clarify that the total thickness of PVB in K4PVB1PE2 is 0.25 mm and in K5PVB2PE2 is 2 × 0.05 = 0.10 mm. Thus, the last sample has 2.5 times less PVB than the first has, and its area density is only slightly more due to an extra layer of Kevlar® fabric. (see Table 1 and Table 2). So, the weaker behavior of K4PVB1PE2 is not surprising. The most important thing is that this causes very significant structural damage, although it is quite localized (Figure 6c). There is also a relatively large bulging of the backside without cracking and fracture. Thus, based on the analysis of all parameters, it can be concluded that the structural combination K5PVB2PE2 performs the best, including protecting against multiple impacts.

5. Conclusions

From the entire analysis above, it should be concluded that the advantages of only one or two properties are not yet sufficient for the overall acceptable behavior of the armor structure. The goal of this work was to optimize the design of a sandwich structure made of Kevlar® fabric, UHMWPE, and PVB to obtain the best combination of three parameters: (1) minimum deformation of the backside of the panel at the moment of impact, (2) minimum absorption of impact energy per areal density, and (3) minimal local destruction of structural integrity. Using Kevlar® fabric (K), UHMWPE (PE), and PVB in the sequence K–PVB–K–PE–K–PE–K–PVB–K demonstrated the best results. Impregnation of Kevlar® fabric with PVB, prevents fibers, yarns, and tows from being pulled out from the woven structure. At the same time, a large number of internal interfaces between PVB and Kevlar fibers prevents the cracks propagation inside the binder polymer. This localizes the irreversible destruction of the composite structure. Several layers of less rigid, but not brittle, easily deformable, and tough UHMWPE in combination with the fabric behind the K–PVB–K sandwich damped the impact, preventing the propagation of brittle failure and absorbing out-of-plane structural deformations. By supplementing the multilayer structure with a sandwich made of K–PVB–K, the same as the front side, we obtained minimal deformation and bulging towards the protected body.
Optimization of such multilayer structures, as well as their interfacial properties, for specific impact energies and impact velocities, is the goal of our current and future research. Based on the logic of the obtained results, thicker layered structures will be tested for ballistic resistance.

Author Contributions

Conceptualization, M.A.N. and D.A.D.; methodology, M.A.N. and D.A.D.; software, N.A.; validation, D.A.D.; formal analysis, D.A.D. and N.A.; investigation, M.A.N., D.A.D., N.A., and O.B.E.; resources, S.P.; data curation, D.A.D.; writing—original draft preparation, D.A.D.; writing—review and editing, D.A.D. and S.P.; supervision, S.P.; project administration, S.P.; funding acquisition, S.P. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the DEVCOM Army Research Laboratory under the Cooperative Agreement No. W911NF-21-2-0007 to Temple University.

Data Availability Statement

The raw data supporting the conclusions of this article will be made available by the authors on request.

Acknowledgments

The authors are grateful to the College of Engineering for financial and resource support through Temple University’s senior design engineer training program, which enabled the construction of the impact device and the use of other equipment.

Conflicts of Interest

The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

References

  1. Ranaweera, P.; Weerasinghe, D.; Fernando, P.L.N.; Raman, S.N.; Mohotti, D. Ballistic Performance of Multi-Metal Systems. Int. J. Prot. Struct. 2020, 11, 379–410. [Google Scholar] [CrossRef]
  2. Fras, T.; Roth, C.C.; Mohr, D. Fracture of High-Strength Armor Steel under Impact Loading. Int. J. Impact Eng. 2018, 111, 147–164. [Google Scholar] [CrossRef]
  3. Yu, Z.; Yang, B.; Chen, X.; Zhang, C.; Guo, F.; Wang, Q.; Cao, W.; Huang, C. Mechanical Anisotropy of Ultra Strong-and-Ductile Lamellar Dual-Phase Steel. J. Mater. Res. Technol. 2024, 28, 3025–3036. [Google Scholar]
  4. Shaikeea, A.J.D.; Cui, H.; O’masta, M.; Zheng, X.R.; Deshpande, V.S. The toughness of mechanical metamaterials. Nat. Mater. 2022, 21, 297–304. [Google Scholar] [CrossRef] [PubMed]
  5. SPatel, K.; Swain, B.K.; Behera, A.; Mohapatra, S.S. Metallic Glasses: A Revolution in Material Science. In Metallic Glasses, Minić, Dragica, Vasić, Milica; Intechopen: Rijeka, Croatia, 2020. [Google Scholar] [CrossRef]
  6. NAndraskar, N.D.; Tiwari, G.; Goel, M.D. Impact response of ceramic structures—A review. Ceram. Int. 2022, 48, 27262–27279. [Google Scholar] [CrossRef]
  7. Zhong, F.; Schwabe, J.; Hofmann, D.; Meier, J.; Thomann, R.; Enders, M.; Mülhaupt, R. All-polyethylene composites reinforced via extended-chain UHMWPE nanostructure formation during melt processing. Polymer 2018, 140, 107–116. [Google Scholar] [CrossRef]
  8. Benzait, Z.; Trabzon, L. A review of recent research on materials used in polymer-matrix composites for body armor application. J. Compos. Mater. 2018, 52, 3241–3263. [Google Scholar] [CrossRef]
  9. Pundhir, N.; Pathak, H.; Zafar, S. Ballistic Impact Performance of Ultra-High Molecular Weight Polyethylene (Uhmwpe) Composite Armour. Sādhanā 2021, 46, 194. [Google Scholar] [CrossRef]
  10. Liang, Y.; Chen, X.; Soutis, C. Review on Manufacture of Military Composite Helmet. Appl. Compos. Mater. 2021, 29, 305–323. [Google Scholar] [CrossRef]
  11. Ballistic Resistance of Body Armor. Nij Standard-0101.06. 2008. Available online: https://nij.ojp.gov/library/publications/ballistic-resistance-body-armor-nij-standard-010106 (accessed on 18 April 2024).
  12. Kevlar® Technical Guide. DuPont. Available online: https://www.dupont.com/content/dam/dupont/amer/us/en/safety/public/documents/en/Kevlar_Technical_Guide_0319.pdf (accessed on 19 February 2024).
  13. Naik, S.; Dandagwhal, R.; Loharkar, P.K. A review on various aspects of Kevlar composites used in ballistic applications. Mater. Today: Proc. 2020, 21, 1366–1374. [Google Scholar] [CrossRef]
  14. Carlsson, D.J.; Gan, L.H.; Wiles, D.M. Photodegradation of Aramids. II. Irradiation in Air. J. Polym. Sci. Polym. Chem. Ed. 1978, 16, 2365–2376. [Google Scholar] [CrossRef]
  15. Zhang, H.; Zhang, J.; Chen, J.; Hao, X.; Wang, S.; Feng, X.; Guo, Y. Effects of solar UV irradiation on the tensile properties and structure of PPTA fiber. Polym. Degrad. Stab. 2006, 91, 2761–2767. [Google Scholar] [CrossRef]
  16. Wei, C.; Qian, X.; He, X.; Liu, J. Enhanced Ultraviolet Resistance of Kevlar Fibers with Tio 2 Films. In Proceedings of the 2011 9th International Conference on Reliability, Maintainability and Safety, Guiyang, China, 12–15 June 2011. [Google Scholar]
  17. Zhang, Z.; Lee, N.; Patel, K.; Young, M.; Zhang, J.; Percec, S.; Ren, S. Poly(P-Phenylene Terephthalamide) Fibers Reinforced with Ultrathin Ceramic Coatings. Adv. Eng. Mater. 2018, 20, 1800095. [Google Scholar] [CrossRef]
  18. Biradar, A.; Arulvel, S.; Kandasamy, J. Significance of ballistic parameters and nanohybridization in the development of textile-based body armor: A review. Int. J. Impact Eng. 2023, 180, 104700. [Google Scholar] [CrossRef]
  19. Wu, S.; Sikdar, P.; Bhat, G.S. Recent progress in developing ballistic and anti-impact materials: Nanotechnology and main approaches. Def. Technol. 2023, 21, 33–61. [Google Scholar] [CrossRef]
  20. Barhoumi, H.; Bhouri, N.; Feki, I.; Baffoun, A.; Hamdaoui, M.; Ben Abdessalem, S. Review of ballistic protection materials: Properties and performances. J. Reinf. Plast. Compos. 2022, 42, 685–699. [Google Scholar] [CrossRef]
  21. Abtew, M.A.; Boussu, F.; Bruniaux, P.; Loghin, C.; Cristian, I. Ballistic impact mechanisms—A review on textiles and fibre-reinforced composites impact responses. Compos. Struct. 2019, 223, 110966. [Google Scholar] [CrossRef]
  22. Hooper, P.A.; Blackman, B.R.K.; Dear, J.P. The mechanical behaviour of poly(vinyl butyral) at different strain magnitudes and strain rates. J. Mater. Sci. 2011, 47, 3564–3576. [Google Scholar] [CrossRef]
  23. Zhang, X.; Hao, H.; Shi, Y.; Cui, J. The mechanical properties of Polyvinyl Butyral (PVB) at high strain rates. Constr. Build. Mater. 2015, 93, 404–415. [Google Scholar] [CrossRef]
  24. Samolov, A.D.; Simić, D.M.; Fidanovski, B.Z.; Obradović, V.M.; Tomić, L.D.; Knežević, D.M. Improvement of VIS and IR camouflage properties by impregnating cotton fabric with PVB/IF-WS2. Def. Technol. 2020, 17, 2050–2056. [Google Scholar] [CrossRef]
  25. Salman, S.D.; Leman, Z.; Sultan, M.T.; Ishak, M.R.; Cardona, F. Ballistic Impact Resistance of Plain Woven Kenaf/Aramid Reinforced Polyvinyl Butyral Laminated Hybrid Composite. BioResources 2016, 11, 7282–7295. [Google Scholar] [CrossRef]
  26. Salman, S.D.; Leman, Z.; Ishak, M.R.; Sultan MT, H.; Cardona, F. Quasi-Static Penetration Behavior of Plain Woven Kenaf/Aramid Reinforced Polyvinyl Butyral Hybrid Laminates. J. Ind. Text. 2018, 47, 1427–1446. [Google Scholar] [CrossRef]
  27. Lee, B.L.; Walsh, T.F.; Won, S.T.; Patts, H.M.; Song, J.W.; Mayer, A.H. Penetration Failure Mechanisms of Armor-Grade Fiber Composites under Impact. J. Compos. Mater. 2001, 35, 1605–1633. [Google Scholar] [CrossRef]
  28. Khan, M.I.; Umair, M.; Hussain, R.; Karahan, M.; Nawab, Y. Investigation of impact properties of para-aramid composites made with a thermoplastic-thermoset blend. J. Thermoplast. Compos. Mater. 2021, 36, 866. [Google Scholar] [CrossRef]
  29. Carpenter, A.J.; Chocron, S.; Scott, N.L.; Anderson, C.E., Jr. Characterization, Modeling, and Ballistic Impact of Kevlar/Phenolic Pvb Composite. J. Dyn. Behav. Mater. 2023, 9, 225–239. [Google Scholar] [CrossRef]
  30. Soykasap, O.; Colakoglu, M. Ballistic performance of a Kevlar-29 woven fibre composite under varied temperatures. Mech. Compos. Mater. 2010, 46, 35–42. [Google Scholar] [CrossRef]
  31. de Ruijter, C.; van der Zwaag, S.; Stolze, R.; Dingemans, T. Liquid crystalline matrix polymers for aramid ballistic composites. Polym. Compos. 2009, 31, 612–619. [Google Scholar] [CrossRef]
  32. Ali, M.F.; Hussain, M.; Tariq, A.; Ahmed, H.I.; Shahid, S.; Saouab, A.; Nawab, Y. Damage-Tolerant Woven Glass Fiber Composites Developed Using Polyvinyl Butyral (PVB) Unsaturated Polyester (UP) Blends. Adv. Mater. Sci. Eng. 2022, 2022, 9077788. [Google Scholar] [CrossRef]
  33. ASTM D7136m-20; Standard Test Method for Measuring the Damage Resistance of a Fiber-Reinforced Polymer Matrix Composite to a Drop-Weight Impact Event. ASTM International: West Conshohocken, PA, USA, 2020.
  34. Mowital® (Polyvinyl Butyral) is a Building Block for Specialty Coatings and Films, Including Trosifol®, Polyvinyl Butyral Film. Kuraray Produces Polyvinyl Butyral (PVB) Resins with Properties That Are Characterized by the Presence of Butyral Units, Hydroxyl, and Acetyl Groups. Kuraray America, Inc. 2024. Available online: https://kuraray.us.com/products/polymers/mowital-piolofor/ (accessed on 3 June 2024).
  35. ASTM D638-10; Standard Test Method for Tensile Properties of Plastics. ASTM International: West Conshohocken, PA, USA, 2015.
  36. ASTM D3763-18; Standard Test Method for High Speed Puncture Properties of Plastics Using Load and Displacement Sensors. ASTM International: West Conshohocken, PA, USA, 2018.
  37. Bai, R.; Ma, Y.; Lei, Z.; Feng, Y.; Liu, D.; Yan, C. Impact resistance analysis of flexible fabric by 3D shape of impact basin in low-speed impact test. Polym. Test. 2020, 81, 106215. [Google Scholar] [CrossRef]
  38. Boumbimba, R.M.; Coulibaly, M.; Khabouchi, A.; Kinvi-Dossou, A.; Bonfoh, N.; Gerard, P. Glass fibres reinforced acrylic thermoplastic resin-based tri-block copolymers composites: Low velocity impact response at various temperatures. Compos. Struct. 2017, 160, 939–951. [Google Scholar] [CrossRef]
  39. Ngan, A.H.W.; Tang, B. Viscoelastic effects during unloading in depth-sensing indentation. J. Mater. Res. 2002, 17, 2604–2610. [Google Scholar] [CrossRef]
  40. Furmanski, J.; Cady, C.M.; Brown, E.N. Time–temperature equivalence and adiabatic heating at large strains in high density polyethylene and ultrahigh molecular weight polyethylene. Polymer 2013, 54, 381–390. [Google Scholar] [CrossRef]
  41. Yakovlev, S.; Fiscus, D.; Brant, P.; Butler, J.; Bucknall, D.G.; Downing, K.H. Mechanism of stress induced crystallization of polyethylene. Polymer 2019, 175, 25–31. [Google Scholar] [CrossRef]
  42. Moreno, C.A.; Piroird, K.; Lorenceau, E. Extended time–temperature rheology of polyvinyl butyral (PVB). Rheol. Acta 2022, 61, 539–547. [Google Scholar] [CrossRef]
Scheme 1. A simplified step-by-step schematic of sample fabrication.
Scheme 1. A simplified step-by-step schematic of sample fabrication.
Polymers 16 01693 sch001
Figure 1. (a) Main components of the home-built impact device. (b) Impactor assembly inside the linear ball bearing (BB) with additional mass (M) and electromagnet armature (AA). (c) Impactor tail (armature) inside the solenoid (S) which is suspended from the pulley. (d) Force sensor (FS) and impactor (IP) attached to the lower end of the assembly. (e) Complete assembly of fasteners and support of the specimen on clay in a backing container. (f) Top view of the container filled with clay (Sargent Art® Plastilina non-hardening modeling clay), shown without the specimen and clamp plate. (g) Cross-sectional drawing showing the fastening of the specimen laying on the backing clay. (h) Truncated cone-shape impactor with the following dimensions: outer diameter OD = 16 mm, tip diameter TD = 1.17 ± 0.05 mm, cone solid angle SA = 85.4°.
Figure 1. (a) Main components of the home-built impact device. (b) Impactor assembly inside the linear ball bearing (BB) with additional mass (M) and electromagnet armature (AA). (c) Impactor tail (armature) inside the solenoid (S) which is suspended from the pulley. (d) Force sensor (FS) and impactor (IP) attached to the lower end of the assembly. (e) Complete assembly of fasteners and support of the specimen on clay in a backing container. (f) Top view of the container filled with clay (Sargent Art® Plastilina non-hardening modeling clay), shown without the specimen and clamp plate. (g) Cross-sectional drawing showing the fastening of the specimen laying on the backing clay. (h) Truncated cone-shape impactor with the following dimensions: outer diameter OD = 16 mm, tip diameter TD = 1.17 ± 0.05 mm, cone solid angle SA = 85.4°.
Polymers 16 01693 g001
Figure 2. The signal from the force sensor during the fall of the impactor, the first impact on the sample (first peak), the rebound, and the second impact (second peak). In the inset, the same signal at an enlarged scale from the moment the fall began until the moment the impactor touched the target. Here, t1 is the moment of release of the impactor, t2 is the escape of the armature from the solenoid, t3 is the moment of contact of the impactor with the sample.
Figure 2. The signal from the force sensor during the fall of the impactor, the first impact on the sample (first peak), the rebound, and the second impact (second peak). In the inset, the same signal at an enlarged scale from the moment the fall began until the moment the impactor touched the target. Here, t1 is the moment of release of the impactor, t2 is the escape of the armature from the solenoid, t3 is the moment of contact of the impactor with the sample.
Polymers 16 01693 g002
Figure 3. Steps of converting the measured (a) force versus time after the impactor has touched the sample, into a change in the (b) velocity of the impactor with time, as it moves and the corresponding (c) displacement (deformation) of the sample under the impactor. (d) The force versus sample displacement (deformation) that corresponds to its damage resistance, and (e) the absorbed energy versus time history. This example is taken from measurements of the PE3K2 sample (see Table 1 and Table 2).
Figure 3. Steps of converting the measured (a) force versus time after the impactor has touched the sample, into a change in the (b) velocity of the impactor with time, as it moves and the corresponding (c) displacement (deformation) of the sample under the impactor. (d) The force versus sample displacement (deformation) that corresponds to its damage resistance, and (e) the absorbed energy versus time history. This example is taken from measurements of the PE3K2 sample (see Table 1 and Table 2).
Polymers 16 01693 g003
Figure 4. Stress–strain behaviors of polymer films having (a) a dumbbell-shape with cartridge paper covering the grip area measured at different strain rates: (b) UHMWPE loaded normal to and (c) along the direction of the roll, (d) UHMWPE measured to 700% strain, rupture didn’t happen, and (e) PVB Mowital® 0.25 mm thick films loaded until fracture.
Figure 4. Stress–strain behaviors of polymer films having (a) a dumbbell-shape with cartridge paper covering the grip area measured at different strain rates: (b) UHMWPE loaded normal to and (c) along the direction of the roll, (d) UHMWPE measured to 700% strain, rupture didn’t happen, and (e) PVB Mowital® 0.25 mm thick films loaded until fracture.
Polymers 16 01693 g004
Figure 5. The impact force versus displacement for samples: (a) K5PE4, (b) K5PVB3, (c) K5PVB2PE2, and (d) K5PVB2PE2 (blue) and K4PVB1PE2 (red). PL—the preloading, RS—the relative stiffness, FZ—the failure stage, ER—the elastic response, Fc—the force of the first crack or damage, Fm—the peak loading force, Rd—the residual deformation at zero loading force.
Figure 5. The impact force versus displacement for samples: (a) K5PE4, (b) K5PVB3, (c) K5PVB2PE2, and (d) K5PVB2PE2 (blue) and K4PVB1PE2 (red). PL—the preloading, RS—the relative stiffness, FZ—the failure stage, ER—the elastic response, Fc—the force of the first crack or damage, Fm—the peak loading force, Rd—the residual deformation at zero loading force.
Polymers 16 01693 g005
Figure 6. Photographs of impact damage front (top row) and back face (bottom row) for four samples: (a) K5PE4, (b) K5PVB3, (c) K4PVB1PE2, and (d) K5PVB2PE2. The scale bar is 6 mm for all images. All photographs were taken from the same angle to visually confirm the size and the depth of damage area on the impact side and the degree of deflection on the reverse side. White dashed lines are for eye guiding.
Figure 6. Photographs of impact damage front (top row) and back face (bottom row) for four samples: (a) K5PE4, (b) K5PVB3, (c) K4PVB1PE2, and (d) K5PVB2PE2. The scale bar is 6 mm for all images. All photographs were taken from the same angle to visually confirm the size and the depth of damage area on the impact side and the degree of deflection on the reverse side. White dashed lines are for eye guiding.
Polymers 16 01693 g006
Figure 7. Absorption of the impactor kinetic energy by the target samples (PE3K2 blue, K5PE4 brown, K5PVB3 green, K5PVB2PE2 red line) (a) as a function of time and (b) as a function of depth from the moment the impactor touches the specimen until it rebounds from it, when the measured force is equal zero. Ei is the initial impact energy, Ee is the elastic energy stored and released, and Ea is the absorbed energy. It is marked with a double-ended arrow only for sample K5P4 (brown curve) for illustration purposes. The ER is the instantaneous elastic sample recovery for sample K5PVB2PE2 (red curve).
Figure 7. Absorption of the impactor kinetic energy by the target samples (PE3K2 blue, K5PE4 brown, K5PVB3 green, K5PVB2PE2 red line) (a) as a function of time and (b) as a function of depth from the moment the impactor touches the specimen until it rebounds from it, when the measured force is equal zero. Ei is the initial impact energy, Ee is the elastic energy stored and released, and Ea is the absorbed energy. It is marked with a double-ended arrow only for sample K5P4 (brown curve) for illustration purposes. The ER is the instantaneous elastic sample recovery for sample K5PVB2PE2 (red curve).
Polymers 16 01693 g007
Table 1. The different composition and stacking sequences of the specimens.
Table 1. The different composition and stacking sequences of the specimens.
IndexStackingNumber of Layers/Kevlar LayersThickness *, mmAreal Density **, kg/m2Heat Press T, °C
PE3K2PE–K–PE–K–PE5/21.34 ± 0.051.00190
K5PE4K–PE–K–PE–K–PE–K–PE–K9/52.62 ± 0.051.84190
K5PVB3 aK–Kpvb–Kpvb–Kpvb–K8/51.39 ± 0.051.37190
K4PVB1PE2 bK–PVB–K–PE–K–PE–K7/41.6 ± 0.11.52190
K5PVB2PE2 cK–PVB–K–PE–K–PE–K–PVB–K9/51.75 ± 0.051.57190
* Measured thickness, ** calculated areal density based on material parameters. a Kevlar® fabric impregnated with PVB, b Mowital® PVB 0.25 mm and c 0.05 mm film thickness.
Table 2. Schematic representation of the cross-sections of the specimen design with relative thickness proportions.
Table 2. Schematic representation of the cross-sections of the specimen design with relative thickness proportions.
PE3K2K5PE4K5PVB3 aK4PVB1PE2 bK5PVB2PE2 c
Polymers 16 01693 i001Polymers 16 01693 i002Polymers 16 01693 i003Polymers 16 01693 i004Polymers 16 01693 i005
UHMWPE (Polymers 16 01693 i006), Kevlar® fabric (Polymers 16 01693 i007), a Kevlar® fabric impregnated with PVB (Polymers 16 01693 i008), b Mowital® PVB 0.25 mm (Polymers 16 01693 i009) and c 0.05 mm (Polymers 16 01693 i010) film thickness.
Table 3. Tensile elastic secant modulus at 3% strain and ultimate tensile strength (UTS) with the corresponding standard deviations for UHMWPE and PVB Mowital® 0.25 mm thick films measured at different loading strain rates and two orthogonal directions for polyethylene.
Table 3. Tensile elastic secant modulus at 3% strain and ultimate tensile strength (UTS) with the corresponding standard deviations for UHMWPE and PVB Mowital® 0.25 mm thick films measured at different loading strain rates and two orthogonal directions for polyethylene.
UHMWPEStrain Rate, %/min
2510
E along, MPa250 ± 3268 ± 3319 ± 3
E normal, MPa286 ± 3348 ± 3380 ± 3
UTS along, MPa14.8 ± 0.215.8 ± 0.217.1 ± 0.2
UTS normal, MPa15.9 ± 0.218.3 ± 0.219.3 ± 0.2
PVB—Mowital®Strain Rate, %/min
21030
E, GPa1.30 ± 0.011.28 ± 0.011.42 ± 0.01
UTS, MPa44.9 ± 0.247.5 ± 0.252.2 ± 0.2
Table 4. The summary of key experimental results of drop-weight tests.
Table 4. The summary of key experimental results of drop-weight tests.
SamplesPeak Force, NPeak Stress, GPaTime to Peak, msFracture Initiation Force, NMaximum Penetration, mmResidual Deformation, mm
PE3K213301.245.68-13.9211.03
K5PE417701.655.00-12.078.14
K5PVB315201.424.04110010.508.23
K4PVB1PE217801.664.0090010.477.79
K5PVB2PE218401.714.24119010.497.33
SamplesFracture Initiation Energy (Total and Per Areal Density)Elastic Energy (Total and Per Areal Density)Absorbed Energy (Total and Per Areal Density)
JJ/(kg/m2)JJ/(kg/m2)JJ/(kg/m2)
PE3K2--0.620.6178.698.69
K5PE4--1.410.777.904.29
K5PVB32.311.680.650.478.666.31
K4PVB1PE21.901.250.930.618.385.52
K5PVB2PE23.141.991.170.758.145.17
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Nael, M.A.; Dikin, D.A.; Admassu, N.; Elfishi, O.B.; Percec, S. Damage Resistance of Kevlar® Fabric, UHMWPE, PVB Multilayers Subjected to Concentrated Drop-Weight Impact. Polymers 2024, 16, 1693. https://doi.org/10.3390/polym16121693

AMA Style

Nael MA, Dikin DA, Admassu N, Elfishi OB, Percec S. Damage Resistance of Kevlar® Fabric, UHMWPE, PVB Multilayers Subjected to Concentrated Drop-Weight Impact. Polymers. 2024; 16(12):1693. https://doi.org/10.3390/polym16121693

Chicago/Turabian Style

Nael, Manal A., Dmitriy A. Dikin, Natnael Admassu, Omar Bahgat Elfishi, and Simona Percec. 2024. "Damage Resistance of Kevlar® Fabric, UHMWPE, PVB Multilayers Subjected to Concentrated Drop-Weight Impact" Polymers 16, no. 12: 1693. https://doi.org/10.3390/polym16121693

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.