Next Article in Journal
High-Reliability Perovskite Quantum Dots Using Atomic Layer Deposition Passivation for Novel Photonic Applications
Next Article in Special Issue
Significantly Suppressed Dielectric Loss and Enhanced Breakdown Strength in Core@Shell Structured Ni@TiO2/PVDF Composites
Previous Article in Journal
Microstructural Analysis of Organic-Rich Shales: Insights from an Electron Microscopic Study by Application of FIBSEM and TEM
Previous Article in Special Issue
Development and Perspectives of Thermal Conductive Polymer Composites
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Understanding the Role of Soft X-ray in Charging Solid-Film and Cellular Electrets

1
School of Mechatronical Engineering, Beijing Institute of Technology, Beijing 100081, China
2
Shanghai Electro-Mechanical Engineering Institute, Shanghai 201109, China
3
Laboratoire Catalyse et Spectrochimie, ENSICAEN, Université de Caen, CNRS, 6 Boulevard Maréchal Juin, 14050 Caen, France
*
Author to whom correspondence should be addressed.
Nanomaterials 2022, 12(23), 4143; https://doi.org/10.3390/nano12234143
Submission received: 25 October 2022 / Revised: 12 November 2022 / Accepted: 14 November 2022 / Published: 23 November 2022

Abstract

:
Solid-film electrets and cellular electrets are defined as promising insulating dielectric materials containing permanent electrostatic and polarizations. High-performance charging methods are critical for electret transducers. Unlike dielectric barrier discharge (DBD) charging, the soft X-ray charging method, with its strong penetration ability, has been widely used in electrets after packaging and has even been embedded in high-aspect-ratio structures (HARSs). However, the related charging model and the charging effect of the soft X-ray irradiation remain unclear. In this study, the charge carrier migration theory and the one-dimensional electrostatic model were employed to build the soft X-ray charging models. The influence of soft X-ray irradiation under deferent poling voltages was investigated theoretically and experimentally. The conducted space charge measurement based on a pulsed electro-acoustic (PEA) system with a soft X-ray generator revealed that soft X-ray charging can offer higher surface charge densities and piezoelectricity to cellular electrets under the critical poling voltage lower than twice the breakdown voltage.

1. Introduction

Permanently charged electrets with a solid film [1,2] or cellular structure [3,4] are insulating dielectric materials that exhibit a net quasi-permanent electrical charge or dipole moment. These electrets carrying trapped charges with strong electrostatic or piezoelectric effects have been widely used in microsystems such as pressure or tactile sensors [5], accelerometers [6], energy harvesters [7,8,9], and actuators [10].
The first electrets were made from natural organics such as carnauba, paraffin, and rosin. However, the low charge densities and poor thermal stabilities of such organic electrets limited their engineering applications. The developed electrets can be classified into inorganic electrets and polymer electrets. Inorganic electrets such as SiO2 and Si3N4 have relatively high charge densities and good compatibility with microelectromechanical system (MEMS) processes. However, the trapped charge of inorganic electrets can easily leak out, resulting in poor charge stability [1,2]. In contrast, polymer electrets, especially fluoropolymer electrets such as polytetrafluoroethylene (PTFE), fluorinated ethylene propylene (FEP), and CYTOPTM, have been widely used in electrostatic transducers because of their high mechanical flexibility, excellent charge stability, and high dielectric breakdown strength [2]. In addition, it was found that the polymer electrets doped with nanoparticles can effectively enhance charge density [11]. Some natural biological tissues such as bone, blood, and skin also exhibit electret effects in the process of human life. These tissue electrets, together with synthetic biocompatible polymers such as PTFE and FEP, are known as bioelectrets [2] that can regulate neural signals, thinking processes, regeneration of biological memory, etc. Recently, the biodegradable electrets [12] represented by polylactic acid (PLA) have attracted interest due to their potential to replace some non-fluorine polymer electrets such as polyethylene (PE) and polypropylene (PP).
Electret films can be prepared by hot pressing or spin coating. In order to precisely control the morphology of the electret at the microscale, MEMS processes, such as chemical vapor deposition (CVD) and etching, are often used to form patterned electrets [10,13,14]. In addition, 3D printing, as a low-cost and rapid manufacturing method, can also print electrets of low melting temperature on flexible substrates [15].
The performance of electret transducers can be determined from the density of charge build-up on the surface layers or internal air voids. High-performance charging methods in the regulation of trapped charges have received great interest. Corona charging [16,17], as a classic unipolar in-air charging method, can easily achieve a high surface charge density on electret surfaces. However, it is incapable of charging electrets after packaging and when embedded in high-aspect-ratio structures (HARSs) because corona ions cannot pass through obstructive substrates and narrow gap openings [13,14,18,19]. The electron beam charging method [20,21] enables a large charging area coverage, as well as localized patterning, but it requires a vacuum environment, and only monopolar charges are deposited. Dielectric barrier discharge (DBD) technology [22,23], which relies on the Paschen breakdown in the air voids caused by an external direct-current (DC) voltage, enables hetero charges to deposit on the internal voids of cellular electrets. However, the inevitable extinguishment of breakdown stops charge transportation, eventually reducing the charging efficiency [22]. To address those issues, Suzuki et al. [13,14,18,19] developed a prospective soft X-ray charging technique in air and revealed the fundamental charging mechanism. Because of the photoionization effect and penetration ability, soft X-rays can be easily transmitted through substrates and generate large amounts of ions in narrow voids, which is rather effective for charging packaged electrets and cellular electrets, even when embedded in HARSs. However, the specific charging models of solid-film and cellular electrets with soft X-ray irradiation remain unclear. In addition, insufficient in situ charge measurements have been provided to demonstrate the charging behaviors of cellular electrets. These aspects are essential to theoretically and experimentally clarify and take full advantage of soft X-ray charging technology.
In this work, we propose a mathematical model of soft X-ray charging to explain the deposition of X-ray irradiated ions on the surface of solid-film electrets and the void surfaces of cellular electrets. The electrification mechanism of soft X-ray charging was interpreted according to the charge carrier migration theory in air dielectric and the one-dimensional electrostatic model of the charged electrets. Importantly, pulsed electro-acoustic (PEA)-based techniques, such as in situ space charge measurement, were employed to describe the charging behaviors of soft X-ray charged cellular electrets. The figures of merit, such as the piezoelectric constant d33 and surface charge density σ, are provided to demonstrate the charging superiority in the comparison between soft X-ray and DBD charging methods.

2. Theoretical Modeling of Soft X-ray Charging Method

2.1. Charging Solid-Film Electrets

Soft X-rays represent short-wavelength (1–10 Å) electromagnetic radiation with photon energies typically below 10 keV, whose interactions with matter are dominated by the photoelectric effect [24]. Figure 1a depicts the mechanism of soft X-ray polarizing electrets, where high-initial-kinetic-energy X-ray photons collide with gas atoms to generate electron–ion pairs as the soft X-rays are irradiated in the air. By applying a high DC as a biased electric field between the top and bottom electrode plates, the positive and negative ions are attracted to the oppositely charged electrodes, and unipolar charges are subsequently transferred to the electret surface.
Soft X-rays are conventionally generated through the processes of field-emission (FE) electron impact on a metal target. The initial X-ray intensity (I0) in the transmitting window of the soft X-ray tube can be calculated using an empirical equation (Equation (1)) [25]:
I 0 = η i X V X 2 Z [ J / s m 2 ]
where η ≈ 1.1–1.4 × 10−9/V is the proportionality coefficient, Z is the atomic number of the target metal, and VX and iX are the tube voltage and tube current of the X-ray generator, respectively.
As illustrated in Figure 1b, the soft X-rays pass through three layers of air (distance L), a top electrode (thickness d), and another air layer (distance H). According to the X-ray attenuation law [26], the X-ray intensity variation (ΔI) due to absorption by air in the gap can be written as:
Δ I = I u p I d o w n = I 0 exp ( μ a i r L μ e d ) [ 1 exp ( μ a i r H ) ]
where μair and μe are the linear absorption coefficients of X-rays in air and the top metal layer, respectively. The amount of electron–ion pairs (nt) generated between the top and bottom electrodes per unit time can be written as:
n t = Δ I S W = I 0 S exp ( μ a i r L μ e d ) [ 1 exp ( μ a i r H ) ] W
where S is the electret area, and W = 33.7 eV is the average ionization energy of the air gas.
The charging current J formed by the directional movement of electrons under the action of the external electric field can be described by the migration–diffusion equation [27]:
J = e n t b E g + e D i n t x
where e is the fundamental charge, Di is the diffusion coefficient, vd = bEg is the driving speed of charge carriers (ions and electrons) under electric field Eg, and the carrier mobility (b) determined by Eg obeys the power law [28]. The Eg in the air gap can be expressed as:
E g = ε 0 ε r V DC σ S h ε 0 ε r H + ε 0 h
where ε0 is the vacuum permittivity, and σS, εr, and h are the surface charge density, relative permittivity, and thickness of the electret, respectively. The variation in surface potential (VS) with charging time (t) can be calculated with respect to the charging current (J):
d V S ( t ) d t = h ε 0 ε r d σ S ( t ) d t = h ε 0 ε r J ( t )
The soft X-ray photoionized charges continuously accumulate on the electret surface, and the effective electric field (Eg) approaches zero. This charge deposition process ends after a sufficient charging time. According to Equations (5) and (6), the amplitude of the maximum surface potential (VS,max) of the electret surface is equal to that of the applied bias voltage VDC.

2.2. Charging Cellular Electrets

Figure 2a gives a schematic diagram of a cellular electret with internally charged voids. The electromechanical operation of cellular electrets is described by a one-dimensional model first proposed by professor Sessler [3]. As described in Figure 2b, a cellular electret consists of N solid electret layers and (N − 1) air layers in thickness hp,i and ha,i, respectively. The electric fields of the ith electret and void are Ep,i and Ea,i, respectively. The permanent charges are assumed to locate only on the void–electret interfaces, and the charges at opposite sides of each void are equal in magnitude when a poling voltage (VDC) is applied.
Based on Gauss’s theorem and Kirchhoff’s second law, the Ea,i in the ith air void can be expressed as [22]:
E a , i = ε 0 ε r V DC σ i i N h p , i ε 0 i N h p , i + ε 0 ε r i N 1 h a , i
In the soft X-ray charging process, charge accumulation on the surfaces of the air voids is nearly terminated, and the strength of the electric field is insufficient to separate ions (i.e., Ea,i = 0). The saturated surface charge density (σi) in the ith void can be written as:
σ i = ε 0 ε r V DC i N h p , i
It is clear that σi cannot increase further when VDC is decreased. In addition, the well-known back discharge effect [22] occurs while Ea,i formed by the trapped charges is higher than the Paschen breakdown field (EDBD). Thus, the maximum surface charge density (σi,max) is derived as:
σ i , max = E DBD ( ε 0 i N h p , i + ε 0 ε r i N 1 h a , i ) i N h p , i
The poling voltage to achieve σi,max is numerically equal to the voltage (VDBD) at which DBD discharge occurs in the ith air void without soft X-ray irradiation:
V DBD = E DBD ( i N h p , i / ε r + ε 0 ε r i N 1 h a , i )
The EDBD of the ith void can be written as follows:
E DBD = A p B + ln ( p h a , i )
where p is the pressure of the air void, and parameter B = ln[C/ln(1 + 1/γ)]. The constants A and C depend on the composition of the gas, and γ is the second ionization coefficient.
The one-dimensional model of the cellular electret can be further simplified to a sandwich structure model with one air layer and two electret layers, where h p = i = 1 N h p , i / 2 and h a = i = 1 N 1 h a , i . The absorption of X-rays in the electret layer can be ignored, and the X-ray ionization rate (nt′) in the air layer can be written as Equation (12). nt′ and Ea were used to calculate the charging current (J) and the surface charge density versus time on the internal void surfaces:
n t = I 0 S exp ( μ a i r L μ e d e μ p h p ) [ 1 exp ( μ a i r h a ) ] W
where μp is the linear absorption coefficients of X-rays in the polymer layer.
Regarding the poling voltage, the theoretical saturation surface charge density in soft X-ray charging can be derived as:
σ X - model - saturation = { ε 0 ε r V DC / 2 h p ε 0 ε r V DBD / 2 h p 0 V DC < V DBD V DC V DBD
Equation (14) is used to describe the surface charge density dependence on poling voltage in the DC DBD charging [4,22,23]:
σ DBD - model = { 0 0 V DC < V DBD ε 0 ε r ( V DC V DBD ) / 2 h p V DBD V DC < 2 V DBD ε 0 ε r V DBD / 2 h p V DC 2 V DBD
According to Equations (13) and (14), there is no charge accumulation on the void interfaces at VDC < VDBD in DBD; in contrast, soft X-ray charging can offer a much higher surface charge density at VDC < 2VDBD. Furthermore, a much lower poling voltage (VDC) is required to achieve σmax in the soft X-ray charging (i.e., VDC = VDBD).

3. Materials and Methods

A commercial soft X-ray generator with a tube voltage of 11.0 kV (SXN-10H, SUNJE electronics, Busan, Republic of Korea) was used to create a high-density plasma. A charging voltage supplier with a large amplitude (−30 to 30 kV) was used to provide a high-level biased electric field between a 15.0 μm-thick aluminum foil as a top electrode and a copper bottom electrode plate with a spacing of 2.0 cm.
A solid-film PTFE electret specimen with a thickness of 500 μm (area of 20 mm × 20 mm) was charged by soft X-ray in the air. Its surface potential was measured with a commercial electrostatic voltmeter (Model 279, Monroe Electronics, Lyndonville, NY, USA). To experimentally describe the charge density on void surfaces of cellular electrets, we employed an in situ space charge measurement method based on the pulsed electro-acoustic (PEA) technique [29,30,31,32] for the cellular electret measurement.
The PEA method is often used to detect charge distribution in solid dielectrics. Figure 3a shows a PEA device for in situ space charge measurement of soft X-ray-charged cellular electrets. Different from traditional PEA devices, our system had the capability of measurement with soft X-ray irradiation. The measurement mechanism was based on the detection of the acoustic waves generated by the vibration of charges inside the specimen after a pulse voltage (pulse width of 20 ns; pulse amplitude of 1400 V) was applied. The generated acoustic waves were detected by a 28 μm-thick polyvinylidene difluoride (PVDF) piezoelectric transducer (LDT0-028K, TE Connectivity, Middletown, CT, USA) and then amplified by a 64 dB-gain low noise amplifier, where the intensity of the signal represented the charge density, and the arrival time of the acoustic wave was used to confirm the positions of the charges inside the specimen.
It should be noted that there is a serious barrier effect [33] of air layers in the process of measuring cellular electrets using PEA systems, which is associated with strong reflections of acoustic waves caused by a large difference in acoustic impedance (Z) between air and electret layers (e.g., Zair = 432 kg/m2s and ZPTFE = 3.15 × 106 kg/m2s). Hence, the prepared cellular electret specimen in the present work only contains a single void rather than multiple voids to ensure a clear signal of charge density distribution. The cellular PTFE specimen comprised a 52.3 μm-thick hollow polyethylene terephthalate (PET) film as a void supporter and two 100 μm-thick PTFE membranes. The voided PTFE electret with 15 μm-thick Al electrode layers had a total thickness of 282.3 μm and an area of 10 mm × 10 mm.
The propagation behaviors of the acoustic waves generated by deposited charges on interfaces are shown in Figure 3b to better understand how the PEA measurement works on cellular electrets. The acoustic waves’ transmission time (τ) in different layers can be calculated as τi = hi/vi, where vi is the sound velocity of related materials (e.g., vPTFE = 1350 m/s in PTFE layers, and vair = 344 m/s in air layers). Here, the moment at which the deposited charges in the PTFE–Al interface resulted in the acoustic wave (marked with I, blue lines in Figure 3b,c) reaching the PVDF sensor is set to 0 ns. After an elapsed time of 74.1 ns, the second wave (marked with II, red lines in Figure 3b,c) arrived due to charge accumulation in the PTFE–air interface. Before receiving the subsequent third wave (wave III associated with the air–PTFE interface, purple lines in Figure 3b,c), two additional waves of non-interest (reflected wave I′ and wave II′) arrived successively. Unfortunately, wave III and reflection wave II′ had a very short time interval (i.e., 3.8 ns), making it difficult to distinguish wave III from the other complex signals. The calculated results are consistent with the experimental results, as shown in Figure 3c. Here, we manually flipped the specimen to obtain clear signals for wave III and wave IV, avoiding the interference of the reflected signals.

4. Results and Discussion

4.1. Solid-Film PTFE Electret

The X-ray ionization rate (nt)-dominated soft X-ray efficiency is mainly influenced by the thickness (d) and linear absorption coefficient (μ) of the top electrode layer. In our facility, the tube voltage (VX), current (iX), and photon energy of the commercial soft X-ray generator using a beryllium (Be) metal target were 11 kV, 200 μA, and 8 keV, respectively. The distance (H) between the top and bottom electrode layers was set to 2 cm, and the X-ray tube was positioned 3 cm above the top electrode layer.
The curves of nt, which were dependent on the thickness of the top electrode layer and calculated from Equations (1)–(3), are depicted in Figure 4a, showing an exponential decay trend. The differences in atomic number and physical density of the aluminum and copper electrodes resulted in different linear absorption coefficients (μ) (i.e., μAl = 135.9 cm−1 in aluminum and μCu = 470.8 cm−1 in copper), where a lower μ means higher X-ray transmission ability through electrode layers with the same thickness, which eventually leads to a higher nt beneath the top aluminum electrode layer.
The numerical relationship between the surface potential (VS) and the X-ray ionization rate (nt) can be obtained from Equations (4)–(6). However, it is difficult to confirm the specified parameters of the field-dependent carrier mobility (b). In this case, experimental data are used to obtain a fitted expression b = kEn of the specimen, where k and n are constants and exponents without physical meaning, respectively. Numerous studies indicated that the properties of the electret, such as dielectric constant, conductivity, thickness, and the ability to trap the ion species, have a great impact on the charging results [11,34,35,36].
Usually, negatively charged electrets tend to have higher surface potential than positively charged electrets under the same conditions [36,37] because some of the electrons cannot attach to air molecules while the charging polarity is negative, and the lightweight electrons are much easier to inject into the specimen rather than on the surface. To reflect the ability of the soft X-ray charging method, the negative-polarity results (blue dots in Figure 4b) were used to fit the mobility (b) as b ( m 2 V 1 s 1 ) = 7.5 E g ( 0.3 0.15 l o g V DC ) × 10 3 . It is clear that the VS of the positively charged specimen has several deviations from the fitted curve using the negative-polarity data.
Figure 5a,b shows the variation in the surface potentials (VS) with the charging time versus poling voltages (VDC). The prediction using the fitted model matches the experimental results well. The VS changed sharply at the beginning and gradually reached saturation with increased charging time. At VDC = ±0.5 kV, ±1.0 kV, ±1.5 kV, and ±2.0 kV, the saturation surface potential VS,max was about ±440 V, ±880 V, ±1350 V, and ±1700 V, respectively. The VS,max could not reach VDC probably because the electric field (Eg) was not sufficient to drive charge injection into the electret as the VS increased. Thus, VS could not further increase, even though Eg had not yet dropped to zero. In addition, the saturation charging time at VDC = ±0.5 kV, ±1.0 kV, ±1.5 kV, and ±2.0 kV was about 7.5 s, 15 s, 25 s, and 32.5 s, respectively.

4.2. Cellular PTFE Electret

It is important to experimentally verify the relationship between the number (N) of electret layers and the surface potential (VS,i) of each electret layer for the soft X-ray-charged cellular PTFE electret. The specimens with N = 2 and 3 were charged at VDC = 1.0 kV for the same charging time of 10 min, as well as the same hp,i = 100.0 μm and ha,i = 1.2 mm. After charging, each electret layer was purposely separated from the assembled cellular electret and measured by Model 279. Figure 6 shows that each electret layer had almost the same surface potential (VS,i), which was approximately equal to VDC/N. For example, the initial VS of surfaces S1, S2, S3, and S4 were about 325 V, −335 V, −330 V, and 320 V, respectively. For the specimen with N = 3, the decay of the deposited hetero-charges showed a relatively good stability for both positive and negative charges within the initial 7 days.
PEA-measured space charge profiles of the soft X-ray-charged cellular PTFE electret with hp = 100.0 μm and ha = 52.3 μm after a charging time of 20 min are shown in Figure 7. Measurements of space charges were carried out after a 5 min short-circuit period. The appearance of hetero-charges density peaks located at the air–PTFE and PTFE–Al interfaces correspond to trapped charges due to the photoionization of soft X-ray-irradiated air. The charge densities continuously increased with increasing VDC and reached saturation when VDC was above 3.0 kV.
The measured surface charge density (σPEA) at the air–PTFE interface was derived from the integral of the PEA-measured space charge density, ρ(x), at the interface region [38]. Figure 8a depicts σ below the poling voltages VDC. For a charging time of 20 min, the soft X-ray-charged specimen (circles on solid lines) exhibited an approximately linear increase in σPEA, and eventually a maximum (σmax = ~0.18 mC/m2) was observed when VDC was over 3 kV. Compared with the DBD charging (σDBD-model, blue dotted line), soft X-ray based cellular electret charging technology was able to generate high-density plasma and enabled higher surface charge densities at the air–PTFE interface, which typically exceeded several times the value in DBD-based charging when VDC < 2 VDBD. Although both σPEA and σDBD-model can eventually achieve the same σmax, the critical poling voltage (VDC) required to reach σmax in soft X-ray was 1.3 VDBD, which meant the soft X-ray charging required a much lower VDC to achieve charging saturation.
Figure 8b illustrates the variation in the surface charge densities (σ) on the top and bottom electret surface layers with the charging time at VDC = 1.0 kV; σ increased rapidly within the first 2 min, and the growth rate gradually slowed down with charging time. The negatively charged top electret surface had a slightly higher charge density than that of the bottom surface. The experimental and the calculated surface charge densities are in good agreement within a short charging time, but obvious differences were observed after 3 min, which can be attributed to insufficient photoionized gas inside the enclosed cellular structure. In addition, as discussed previously, it is impossible to reach the theoretical saturation (σ) because charge carriers require a sufficient electric field to be injected into the electret layer.
The piezoelectric constant d33—as a figure of merit to indicate the piezoelectric response of cellular electrets—was given with respect to the surface charge density. The theoretical value of d33 was determined in References 4, 14, 22, and 23. The effective Young’s modules (Y) of the cellular PTFE electret was estimated to be 1.3 MPa. The quasi-static method is a direct method to assess d33. As shown in Figure 9, a lightweight pre-load was used to hold the cellular electret specimen, and external force was applied or removed along the thickness direction of the specimen through a mass (M) of 20.05 g. The amount of charges (Q) generated by the specimen was determined using a fabricated charge meter (INA 128, Texas Instruments, USA). The relationship between quasi-static d33 and generated Q can be expressed as Q = Mg·d33. The measurement results of quasi-static d33 (circles, solid line shown in Figure 9) describe a similar tendency as the surface charge density versus poling voltages. The obtained maximum d33 was about 150 pC/N. This finding further verifies that the soft X-ray charging method can achieve a high piezoelectricity at a lower charging voltage (VDC) (e.g., VDC < 2 VDBD).

5. Conclusions

In this paper, charging models and charging behaviors are analyzed with respect to soft X-ray charging for both solid-film and cellular electrets. The soft X-ray charging model, associated with the electrostatic model, is proposed based on the theories of X-ray photoionization and charge carrier migration diffusion. Well-fitted models are useful to predict the charging preference and understand the role of soft X-ray in charging. Importantly, the surface charge density on the internal voids of the cellular electret was measured in situ using a PEA-based system with soft X-ray irradiation. The soft X-ray-charged cellular electrets required a much lower poling voltage to achieve saturation than that in the DBD charging method. The critical poling voltages of the maximum surface charge density and piezoelectricity were 1.3 VDBD and 2 VDBD for soft X-ray charging and DBD charging, respectively. These findings are significant to better understanding the mechanism and application of the soft X-ray charging method in electrets and electret transducers.

Author Contributions

Conceptualization, Y.F.; methodology, Y.F., Z.R. and X.T.; validation, Y.F. and Z.R.; formal analysis, Y.F., Z.R. and Z.Z.; investigation, Z.R., X.T., Z.Z., K.-Y.S. and Y.X.; resources, Y.F.; writing Y.F., Z.R. and K.-Y.S.; supervision, Y.F. and Y.X.; project administration, Y.F.; funding acquisition, Y.F. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Natural Science Foundation of China, grant number 52077005.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data are contained within the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Li, X.; Wang, Y.; Xu, M.; Shi, Y.; Wang, H.; Yang, X.; Ying, H.; Zhang, Q. Polymer electrets and their applications. J. Appl. Polym. Sci. 2021, 138, 50406. [Google Scholar] [CrossRef]
  2. Sessler, G.M. Electrets, 2nd ed.; Springer: Berlin, Germany, 1987. [Google Scholar]
  3. Hillenbrand, J.; Sessler, G.M. Piezoelectricity in cellular electret films. IEEE Trans. Dielect. Electr. Insul. 2000, 7, 537–542. [Google Scholar] [CrossRef]
  4. Qiu, X.; Bian, Y.; Liu, J.; Xiang, Y.; Ding, T.; Zhu, W.; Xuan, F.Z. Ferroelectrets: Recent developments. IET Nanodielectr. 2022, 1–12. [Google Scholar] [CrossRef]
  5. Tao, K.; Chen, Z.; Yi, H.; Zhang, R.; Shen, Q.; Wu, J.; Tang, L.; Fan, K.; Fu, Y.; Miao, J.; et al. Hierarchical honeycomb-structured electret/triboelectric nanogenerator for biomechanical and morphing wing energy harvesting. Nano-Micro Lett. 2021, 13, 123. [Google Scholar] [CrossRef] [PubMed]
  6. Hillenbrand, J.; Motz, T.; Sessler, G.M. High sensitivity electret accelerometer with integrated FET. IEEE Sens. J. 2014, 14, 1770–1777. [Google Scholar] [CrossRef]
  7. Feng, Y.; Zhou, Z.; Fu, D.; Ren, W. Velocity-amplified monostable dual-charged electret dome energy harvester using low-speed finger tapping. Appl. Phys. Lett. 2020, 116, 063905. [Google Scholar] [CrossRef]
  8. Ma, X.; Yang, X.; von Seggern, H.; Dai, Y.; He, P.; Sessler, G.M.; Zhang, X. Tuneable resonance frequency vibrational energy harvester with electret-embedded variable capacitor. IET Nanodielectr. 2021, 4, 53–62. [Google Scholar] [CrossRef]
  9. Feng, Y.; Yu, Z.; Han, Y. High-performance gap-closing vibrational energy harvesting using electret-polarized dielectric oscillators. Appl. Phys. Lett. 2018, 112, 032901. [Google Scholar] [CrossRef]
  10. Sano, C.; Ataka, M.; Hashiguchi, G.; Toshiyoshi, H. An electret-augmented low-voltage MEMS electrostatic out-of-plane actuator for acoustic transducer applications. Micromachines 2020, 11, 267. [Google Scholar] [CrossRef] [Green Version]
  11. Kim, S.; Suzuki, K.; Sugie, A.; Yoshida, H.; Yoshida, M.; Suzuki, Y. Effect of end group of amorphous perfluoro-polymer electrets on electron trapping. Sci. Technol. Adv. Mater. 2018, 19, 486–494. [Google Scholar] [CrossRef] [PubMed]
  12. Zhukov, S.; Ma, X.; Seggern, H.V.; Sessler, G.M.; Dali, O.B.; Kupnik, M.; Zhang, X. Biodegradable cellular polylactic acid ferroelectrets with strong longitudinal and transverse piezoelectricity. Appl. Phys. Lett. 2020, 117, 112901. [Google Scholar] [CrossRef]
  13. Hagiwara, K.; Goto, M.; Iguchi, Y.; Tajima, T.; Yasuno, Y.; Kodama, H.; Kidokoro, K.; Suzuki, Y. Electret charging method based on soft X-ray photoionization for MEMS transducers. IEEE Trans. Dielect. Electr. Insul. 2012, 19, 1291–1298. [Google Scholar] [CrossRef]
  14. Feng, Y.; Hagiwara, K.; Iguchi, Y.; Suzuki, Y. Trench-filled cellular parylene electret for piezoelectric transducer. Appl. Phys. Lett. 2012, 100, 262901. [Google Scholar] [CrossRef]
  15. Kierzewski, I.; Bedair, S.S.; Hanrahan, B.; Tsang, H.; Hu, L.; Lazarus, N. Adding an electroactive response to 3D printed materials: Printing a piezoelectret. Addit. Manuf. 2020, 31, 100963. [Google Scholar] [CrossRef]
  16. Gulyakova, A.A.; Galikhanov, M.F.; Ma, X.; Zhang, X.; Fang, P. The Peculiarities of Electret Effect in Corona Electrets Based on Nonpolar and Polar Polymers with Dispersed Montmorillonite. IEEE Trans. Dielect. Electr. Insul. 2022, 29, 840–844. [Google Scholar] [CrossRef]
  17. Moreno, R.A.; Gross, B. Measurement of potential buildup and decay, surface charge density, and charging currents of corona-charged polymer foil electrets. J. Appl. Phys. 1976, 47, 3397–3402. [Google Scholar] [CrossRef]
  18. Hagiwara, K.; Goto, M.; Iguchi, Y.; Yasuno, Y.; Kodama, H.; Kidokoro, K.; Tajima, T. Soft X-ray charging method for a silicon electret condenser microphone. Appl. Phys. Express 2010, 3, 091502. [Google Scholar] [CrossRef]
  19. Lu, J.; Suzuki, Y. Push-button kinetic energy harvester with soft-x-ray-charged folded multilayer piezoelectret. J. Phys. Conf. Ser. 2019, 1407, 012021. [Google Scholar] [CrossRef]
  20. Wu, M.L.; Wang, D.; Wan, L.J. Directed block copolymer self-assembly implemented via surface-embedded electrets. Nat. Commun. 2016, 7, 10752. [Google Scholar] [CrossRef] [Green Version]
  21. Bonacci, F.; Di Michele, A.; Caponi, S.; Cottone, F.; Mattarelli, M. High charge density silica micro-electrets fabricated by electron beam. Smart Mater. Struct. 2018, 27, 075052. [Google Scholar] [CrossRef]
  22. Qiu, X.; Gerhard, R.; Mellinger, A. Turning polymer foams or polymer-film systems into ferroelectrets: Dielectric barrier discharges in voids. IEEE Trans. Dielect. Electr. Insul. 2011, 18, 34–42. [Google Scholar] [CrossRef]
  23. Zhukov, S.; Eder-Goy, D.; Biethan, C.; Fedosov, S.; Xu, B.X.; von Seggern, H. Tubular fluoropolymer arrays with high piezoelectric response. Smart Mater. Struct. 2017, 27, 015010. [Google Scholar] [CrossRef]
  24. Attwood, D. Soft X-rays and Extreme Ultraviolet Radiation: Principles and Applications; Cambridge University Press: Cambridge, UK, 2000. [Google Scholar]
  25. Ooka, M.; Sasaoka, H.; Nishimura, K. An X-ray generator using nano-diamond field emission devices. J. Jpn. Soc. Abras. Technol. 2007, 51, 725–728. [Google Scholar] [CrossRef]
  26. Jackson, D.F.; Hawkes, D.J. X-ray attenuation coefficients of elements and mixtures. Phys. Rep. 1981, 70, 169–233. [Google Scholar] [CrossRef]
  27. Kang, W.S.; Park, J.M.; Kim, Y.; Hong, S.H. Numerical study on influences of barrier arrangements on dielectric barrier discharge characteristics. IEEE Trans. Plasma Sci. 2003, 31, 504–510. [Google Scholar] [CrossRef] [Green Version]
  28. Wintle, H.J. Surface-charge decay in insulators with nonconstant mobility and with deep trapping. J. Appl. Phys. 1972, 43, 2927–2930. [Google Scholar] [CrossRef]
  29. Imburgia, A.; Miceli, R.; Sanseverino, E.R.; Romano, P.; Viola, F. Review of space charge measurement systems: Acoustic, thermal and optical methods. IEEE Trans. Dielect. Electr. Insul. 2016, 23, 3126–3142. [Google Scholar] [CrossRef]
  30. Umran, H.M.; Wang, F.; He, Y. Ageing: Causes and effects on the reliability of polypropylene film used for HVDC capacitor. IEEE Access 2020, 8, 40413–40430. [Google Scholar] [CrossRef]
  31. Zhai, J.; Li, W.; Zha, J.; Cheng, Q.; Bian, X.; Dang, Z. Space charge suppression of polyethylene induced by blending with ethylene-butyl acrylate copolymer. CSEE J. Power Energy Syst. 2019, 6, 152–159. [Google Scholar] [CrossRef]
  32. Li, Z.; Su, J.; Du, B.; Hou, Z.; Han, C. Inhibition Effect of Graphene on Space Charge Injection and Accumulation in Low-Density Polyethylene. Nanomaterials 2018, 8, 956. [Google Scholar] [CrossRef]
  33. Imburgia, A.; Romano, P.; Rizzo, G.; Viola, F.; Ala, G.; Chen, G. Reliability of PEA Measurement in Presence of an Air Void Defect. Energies 2020, 13, 5652. [Google Scholar] [CrossRef]
  34. Komeijani, A.; Bagheri, H.; Shekarchi, B. Surface potential uniformity and sensitivity of large-area PTFE electret discs of different thicknesses produced by a modified corona poling rotating system for dosimetry applications. J. Adv. Dielectr. 2019, 9, 1950050. [Google Scholar] [CrossRef] [Green Version]
  35. Jiang, P.; Zhao, X.; Li, Y.; Liao, Y.; Hua, T.; Yin, X.; Yu, J.; Ding, B. Moisture and oily molecules stable nanofibrous electret membranes for effectively capturing PM2. 5. Compos. Commun. 2017, 6, 34–40. [Google Scholar] [CrossRef]
  36. Vu-Cong, T.; Jean-Mistral, C.; Sylvestre, A. Electrets substituting external bias voltage in dielectric elastomer generators: Application to human motion. Smart Mater. Struct. 2013, 22, 025012. [Google Scholar] [CrossRef]
  37. Diniş, C.M.; Popa, G.N. Experimental analysis of direct current corona discharge. IOP Conf. Ser. Mater. Sci. Eng. 2017, 163, 012035. [Google Scholar] [CrossRef] [Green Version]
  38. Vu, T.T.N.; Teyssedre, G.; Le Roy, S.; Laurent, C. Maxwell–Wagner effect in multi-layered dielectrics: Interfacial charge measurement and modelling. Technologies 2017, 5, 27. [Google Scholar] [CrossRef]
Figure 1. Soft X-ray charging solid-film electrets: (a) schematic of dynamic behavior of ions; (b) equivalent electrical model.
Figure 1. Soft X-ray charging solid-film electrets: (a) schematic of dynamic behavior of ions; (b) equivalent electrical model.
Nanomaterials 12 04143 g001
Figure 2. Soft X-ray charging cellular electrets. (a) Schematic of cellular electret; (b) One-dimensional model.
Figure 2. Soft X-ray charging cellular electrets. (a) Schematic of cellular electret; (b) One-dimensional model.
Nanomaterials 12 04143 g002
Figure 3. In situ PEA measurement of the space charge for X-ray irradiated cellular electret. (a) Experimental setup of PEA system. (b) Calculated acoustic waves transmission in the prepared cellular PTFE electret. (c) Electrical response signal received by a PVDF sensor.
Figure 3. In situ PEA measurement of the space charge for X-ray irradiated cellular electret. (a) Experimental setup of PEA system. (b) Calculated acoustic waves transmission in the prepared cellular PTFE electret. (c) Electrical response signal received by a PVDF sensor.
Nanomaterials 12 04143 g003
Figure 4. The metal materials influenced the soft X-ray ionization rate and the charging performance: (a) ionization rates beneath the electrode layer; (b) obtained surface potentials after a charging time of 10 s at VDC = ±2.00 kV.
Figure 4. The metal materials influenced the soft X-ray ionization rate and the charging performance: (a) ionization rates beneath the electrode layer; (b) obtained surface potentials after a charging time of 10 s at VDC = ±2.00 kV.
Nanomaterials 12 04143 g004
Figure 5. Surface potential of soft X-ray charging PTFE electret. (a) Positive charge deposition; (b) Negative charge deposition.
Figure 5. Surface potential of soft X-ray charging PTFE electret. (a) Positive charge deposition; (b) Negative charge deposition.
Nanomaterials 12 04143 g005
Figure 6. Surface potential of each electret layer inside cellular PTFE electret after soft X-ray charging at VDC = 1.00 kV. (a) Specimen with N = 2; (b) Specimen with N = 3.
Figure 6. Surface potential of each electret layer inside cellular PTFE electret after soft X-ray charging at VDC = 1.00 kV. (a) Specimen with N = 2; (b) Specimen with N = 3.
Nanomaterials 12 04143 g006
Figure 7. Measured space charge distribution of cellular PTFE electrets.
Figure 7. Measured space charge distribution of cellular PTFE electrets.
Nanomaterials 12 04143 g007
Figure 8. Surface charge densities (σ) of soft X-ray-charged cellular electret. (a) The dependence of σ on the poling voltage (VDC); (b) The dependence of σ on charging time at VDC = 1.00 kV.
Figure 8. Surface charge densities (σ) of soft X-ray-charged cellular electret. (a) The dependence of σ on the poling voltage (VDC); (b) The dependence of σ on charging time at VDC = 1.00 kV.
Nanomaterials 12 04143 g008
Figure 9. The dependence of quasi-static d33 on the poling voltage (VDC) in cellular PTFE electrets.
Figure 9. The dependence of quasi-static d33 on the poling voltage (VDC) in cellular PTFE electrets.
Nanomaterials 12 04143 g009
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Feng, Y.; Rao, Z.; Song, K.-Y.; Tang, X.; Zhou, Z.; Xiong, Y. Understanding the Role of Soft X-ray in Charging Solid-Film and Cellular Electrets. Nanomaterials 2022, 12, 4143. https://doi.org/10.3390/nano12234143

AMA Style

Feng Y, Rao Z, Song K-Y, Tang X, Zhou Z, Xiong Y. Understanding the Role of Soft X-ray in Charging Solid-Film and Cellular Electrets. Nanomaterials. 2022; 12(23):4143. https://doi.org/10.3390/nano12234143

Chicago/Turabian Style

Feng, Yue, Zehong Rao, Ki-Young Song, Xusong Tang, Zilong Zhou, and Ying Xiong. 2022. "Understanding the Role of Soft X-ray in Charging Solid-Film and Cellular Electrets" Nanomaterials 12, no. 23: 4143. https://doi.org/10.3390/nano12234143

APA Style

Feng, Y., Rao, Z., Song, K. -Y., Tang, X., Zhou, Z., & Xiong, Y. (2022). Understanding the Role of Soft X-ray in Charging Solid-Film and Cellular Electrets. Nanomaterials, 12(23), 4143. https://doi.org/10.3390/nano12234143

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.