Next Article in Journal
Low Impact Velocity Modeling of 3D Printed Spatially Graded Elastomeric Lattices
Next Article in Special Issue
Effects of Polyoxymethylene Fiber on Fresh and Hardened Properties of Seawater Sea-Sand Concrete
Previous Article in Journal
Removal Efficiency of Sulfapyridine from Contaminated Surface Water by Carboxylated Graphene Oxide Blended PVDF Composite Ultrafiltration Membrane with Activated Carbon
Previous Article in Special Issue
Axial Compression Property Test of GFRP Tube-Confined Coal Gangue Steel Fiber Short Concrete Column
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Review

Anti-Corrosion Reinforcements Using Coating Technologies—A Review

1
State Key Laboratory of Mountain Bridge and Tunnel Engineering, Chongqing Jiaotong University, Chongqing 400074, China
2
School of Civil Engineering, Chongqing Three Gorges University, Chongqing 404100, China
3
School of Civil Engineering, Chongqing University, Chongqing 400045, China
4
School of Management Science and Real Estate, Chongqing University, Chongqing 400045, China
*
Author to whom correspondence should be addressed.
Polymers 2022, 14(21), 4782; https://doi.org/10.3390/polym14214782
Submission received: 26 September 2022 / Revised: 17 October 2022 / Accepted: 1 November 2022 / Published: 7 November 2022
(This article belongs to the Special Issue Advances in Fiber-Reinforced Polymer Concrete)

Abstract

:

Highlights

What are the main findings?
  • Anti-corrosion reinforcements, including galvanized reinforcements, epoxy coated reinforcements, stainless cladding reinforcements and steel-fiber reinforced polymer composite bars, are reviewed.
  • The impacts of the manufacturing process and material properties on the performance of anti-corrosion reinforcements are reviewed.
  • The behaviors of anti-corrosion reinforcements, with and without corrosion, are described in detail.
  • The development and application of anti-corrosion reinforcements are introduced.
What is the implication of the main finding?
  • The anti-corrosion reinforcements conform to the development of modern structures.

Abstract

Coated reinforcements are expected to improve the performance of reinforced concrete in aggressive environments, but different kinds of coated reinforcements can express a variety of properties, which can confuse researchers and engineers. This paper reviews the manufacture, corrosion mechanisms, behaviors, and applications of popular or promising coated reinforcements, incorporating galvanized reinforcements (GRs), epoxy coated reinforcements (ECRs), stainless cladding reinforcements (SCRs), and steel-fiber reinforced polymer composite bars (SFCBs). In terms of manufacture, GRs and ECRs should focus on minimizing the negative effect of manufacture on performance, while SCRs and SFCBs should reduce the cost and increase the production capacity. Behaviors of GRs and ECRs are primarily determined by the steel substrate, but the behaviors of SCRs and SFCBs are primarily affected by the coat and core, and their interaction. The corrosion mechanism of GRs and SCRs is about oxidation, while that of SFCBs is about hydrolysis. ECRs are usually corroded under film, which can be a cause of premature failure. Corrosion embrittles SCRs, as well as bare bars, but corrosion of SFCBs usually causes a reduction in maximum strength. The investigation of the corrosion behaviors of GRs and ECRs focuses on bond strength. GRs have controversial performance. ECRs have been proven to have drawbacks regarding bond strength. The use of anti-corrosion reinforcement is uneven in regions, which may correlate with the development of technology and the economy.

1. Introduction

Concrete is one of the most common materials for construction in the world [1]. Its strong compressive strength and economic cost offer a solution for most structural requirements. To enhance tensile ability and serviceability, concrete is always reinforced with steel reinforcements [2]. The good interaction between steel and concrete ensures that reinforced concrete exhibits the advantages of both. However, as detection of corrosive damages to construction built in the last century has become increasingly apparent, the challenges of dealing with corrosion require addressing [3]. Corrosion not only degrades the strength and ductility of the reinforcements, but also reduces the fatigue performance and bond strength. Thereby, the mechanical performance and serviceability of structures are compromised, typical signs of which include intensive cracks, large deflection, and even brittle failure. In the USA, the annual direct corrosion cost of highway bridges alone was about $8.3 billion in 2014 [4]. The American Society of Civil Engineering predicts that infrastructural repair will cost about $2 trillion by 2025 [5]. In China, the cost of reinforcement corrosion is about 1.2% of its Gross Domestic Product, which exceeded $2 trillion in 2021 [6].
To prevent corrosion in reinforced concrete structures, several practical applications are available, including concrete protective coatings, corrosion inhibitors, cathodic protection, and anti-corrosion reinforcement. Concrete protective coating enhances the civil life of a structure by blocking the penetration of detrimental elements, but the duration of effective protection is still less than the design lifetime of the structure [7,8,9,10]. The use of corrosion inhibitors could be a solution, but they may degrade the mechanical properties of concrete [11,12,13]. Cathodic protection is an effective method; however, it is expensive and difficult to install in some scenarios [2,14,15]. Anti-corrosion reinforcements are recognized as effective and practical ways to expand the lifetimes of structures in either normal or aggressive environments [8,16,17].
As shown in Figure 1, there are numerous publications on anti-corrosion. Coating technology is a common way to resist corrosion [18,19,20,21,22]. In this paper, the research hot spots in the field of anti-corrosion reinforcements using coating technologies were studied by bibliometric analysis. Papers that contained the keywords “galvanized reinforcement”, “epoxy coated reinforcement”, “stainless cladding reinforcement”, and “steel-FRP composite bar” were extracted from the Web of Science Core Collection. The open-source software program Citespace 5.8.R3 was used to analyze data and visualize results [23,24,25,26]. As shown in Figure 2, papers written earlier mainly focused on mechanical properties and behaviors of GRs and ECRs without corrosion, and bond strength was highly emphasized. Since 2000, when anti-corrosion coatings and composite bars (such as SCRs and SFCBs) were invented, studies about corrosion behaviors began to emerge. Thus, this paper introduces the mechanical performance (tensile, fatigue, and bond behaviors) of GRs, ECRs, SCRs, and SFCBs, with particular emphasis on the effects of manufacture and corrosion. Then, applications and future works are addressed.
The development of the review on reinforcements is shown in Figure 3. Galvanized reinforcement (GR) has been applied to construction since the 1930s [27], in which zinc serves as the coating, providing cathodic protection for steel. In the USA, de-icing salt was widely used in highway bridges in the 1960s, since bridge decks demand higher corrosion resistance at an acceptable cost [28]. Epoxy coated reinforcement (ECR) was developed and used in highway constructions in the 1970s [3,27,28,29]. However, as more cases of corroded epoxy coated reinforcements have been reported since the 1990s [3,28,30,31], the protection effectiveness of the epoxy coat has become controversial. To further improve the anti-corrosion and mechanical performance of reinforcements, stainless cladding reinforcement (SCR) and steel-FRP composite bars (SFCBs) were introduced in the 1990s and 2000s [32,33,34,35,36,37,38,39,40,41], respectively. These reinforcements were founded on the reliable corrosion resistance of stainless steel and FRP. In practice, SCR has been adopted in certain infrastructures since the 2000s [42,43], but the application of SFCBs remains deficient.
Current reviews study novel methods to enhance corrosion resistance or focus on one type of anti-corrosion coating and its application [18,19,20,21,22,44,45,46,47,48,49,50]. Specifically, Ding [48] reviewed the improvements offered by using graphene in organic anti-corrosion coatings. Lazorenko et al. [49] reviewed anti-corrosion coatings, including organic, inorganic, metallic and combined coatings, in the protection of steel railway structures from atmospheric corrosion. In terms of coated reinforcements, Zemajtis [28] reviewed the performance of bridges reinforced by epoxy coated reinforcements. Yeomans [16] presented an overview of galvanized reinforcements. Sun et al. [50] summarized the behaviors of SFCBs and structures reinforced by SFCBs. However, SCRs have not been reviewed, even though they have had wide applications. Furthermore, there are only rare reviews comparing the mechanical properties and behaviors, with and without corrosion, of multiple anti-corrosion coating technologies. Yet a comparison is necessary for the popularization and development of anti-corrosion reinforcements using coating technologies. Thus, this review aimed to comprehensively compare the most popular coating technologies that apply to reinforcements and to explore the value of anti-corrosion reinforcements in civil construction.
Figure 1. The publication analysis on anti-corrosion: (a) patents and (b) cited works in recent years [51,52].
Figure 1. The publication analysis on anti-corrosion: (a) patents and (b) cited works in recent years [51,52].
Polymers 14 04782 g001
Figure 2. Combined frequency and centrality of keywords (the size of cycle and width of line represent the frequency and centrality).
Figure 2. Combined frequency and centrality of keywords (the size of cycle and width of line represent the frequency and centrality).
Polymers 14 04782 g002
Figure 3. The development of anti-corrosion reinforcements using coating technologies [3,27,28,29,30,31,32,33,34,35,36,37,38,39,40,41,42,43].
Figure 3. The development of anti-corrosion reinforcements using coating technologies [3,27,28,29,30,31,32,33,34,35,36,37,38,39,40,41,42,43].
Polymers 14 04782 g003

2. Manufacture

Over the past century, GRs have been widely investigated as an alternative coating to protect steel from corrosion [16,53]. GR is generally formed by having a zinc layer, metallurgical layer, and base steel. There are varying ways to coat zinc on the surface of the steel, one of which, the hot-dip method, is recognized as being an economical technology [2]. As shown in Table 1, zinc has lower strength and elastic modulus than steel, and, regarding coating thickness, the zinc layer is usually thin. Thus, the steel substrate dominates the tensile properties of bars. The hot-dip method has negligible influence on the mechanical properties of normal and low strength grade bars because the bars have not been excessively cold worked during fabrication. High strength bars may exhibit slight improvements in strength and ductility, due to minor stress relief. Cold-twisted steel bars can be embrittled by the hot-dip method [53,54].
The manufacture of epoxy coating on bars includes methods such as spray-on, dipped-in, shelling, and electrostatic spraying; the most common of which is electrostatic spraying [55,56]. As shown in Table 1, epoxy coating generally has an insignificant influence on the basic mechanical property of reinforcement, due to its low strength, stiffness and minor thickness. However, an early report pointed out that the epoxy coating may slightly embrittle the reinforcement [31].
Since the 1990s, researchers have shown an increasing interest in SCRs [33,34,35]. The behaviors of SCRs are affected by cladding and core, and their interaction. Since the properties of stainless steel and steel have similarities, which are shown in Table 1, their interaction becomes an important issue to ensure the composite action of the two materials. Hot-rolling is an effective technology to achieve proper interaction by forming a metallurgical bond between steel and stainless steel [33,57,58,59]. With increase in rolling temperature, the promotion of strength becomes more distinct [58]. However, early hot-rolling SCR still had problems of insufficient rib height, de-bonding between the coating and core, and expensive costs [32,60]. In 2015, Hunan 3T New Materials CO., LTD., produced the stainless-clad bimetallic steel bar (SCBSB) by continuous hot rolling with a net interfacial compound [60]. The corrosion resistance and mechanical properties of SCRs were guaranteed.
SFCB improves the performance of steel reinforcement by winding fibers around the rebar [36,37,61]. The fiber used is well-known for its use in FRP. Technically, the rust and longitude ribs of the steel substrate are removed. Then, the bar is wound by the roving that fills the gaps between the ribs. The above measures ensure that the FRP layer bonds well with the steel bar. Unlike previous coated bars, the protective coat of SFCBs plays a distinct part in the tensile behavior of reinforcement because of having higher strength and thicker coating than GRs and ECRs, as shown in Table 1 [36,50,62,63]. The FRP coat can be made from carbon fiber reinforced polymer (CFRP), glass fiber reinforced polymer (GFRP), or basalt fiber reinforced polymer (BFRP). BFRP is mainly recommended [36,62,63,64].
Table 1. Properties of components of coated reinforcements.
Table 1. Properties of components of coated reinforcements.
ItemElastic Modulus
(GPa)
Yield
Strength
(MPa)
Tensile Strength (MPa)Density
(g/cm3)
Elongation
Rate
(%)
Coating Thickness (mm)Refs.
BSR200276~517483~6907.856~12-[65,66]
Zinc10875-7.14-0.085~0.087[16,67]
Epoxy22~35-100~2201.2-0.13~0.23[3,30]
Basalt fiber (CBF13)90-22502.632.52.1~3.4[36]
Resin
(Atlac 430)
3.6-951.066.1-[36]
S30408204>2055207.93 35 1.7~3.1[33,68]

3. Behavior without Corrosion

3.1. Tensile Properties

The tensile properties of anti-corrosion reinforcements are summarized in Table 2, and Figure 4 draws the typical strain–stress curve of anti-corrosion reinforcements. In general, the elastic modulus, ductility, and failure modes were compared, but the values of yield strengths and ultimate strengths are not discussed here, because different steels are adopted. Specifically, galvanized reinforcements (GRs), epoxy coated reinforcements (ECRs), and stainless cladding reinforcements (SCRs) have similar elastic modulus and failure mode to black steel reinforcements (BSRs), where ductile fracture is usually observed. The stress of SFCB continues to increase linearly after steel yielding because of the high strength of the fiber. There is a sudden drop of stress after fiber rupture but the steel prevents full stress dissipation. As shown in Table 2, the coating and core of SFCBs show different failure behaviors, which are blow-out fracture and ductile fracture, respectively. In contrast, SCRs show ductile fracture, and stainless steel cladding and steel substrate still bond well after the has been SCR necked. SCR has enhanced ductility, over other reinforcements, because stainless steel is more ductile than black steel.
Table 2. Tensile properties of reinforcements.
Table 2. Tensile properties of reinforcements.
ItemElastic Modulus (GPa)ElongationFailure ModeRefs.
BSR2000.06~0.12Polymers 14 04782 i001[65,66,69]
GR1920.11~0.16Similar to bare bar, steel substrate dominates the failure mode.[27,54,70]
ECR1920.11~0.14Polymers 14 04782 i002[27,31,71]
SCR185~1960.22~0.24Polymers 14 04782 i003[33,57,60,72,73]
SFCB123~1680.15Polymers 14 04782 i004[36,37,39,62,63]
Note: black steel reinforcement (BSR); galvanized reinforcement (GR); epoxy coated reinforcement (ECR); stainless cladding reinforcement (SCR); steel-FRP composite bar (SFCB).
Figure 4. Comparison of typical tensile properties of GR [70], ECR [27], SCR [74], and SFCB [75].
Figure 4. Comparison of typical tensile properties of GR [70], ECR [27], SCR [74], and SFCB [75].
Polymers 14 04782 g004

3.2. Fatigue Properties

In coastal constructions, seismic performance is always considered because plate activity is relatively active in coastal areas. Coastal areas also need anti-corrosion reinforcements. As confirmed by Sheng and Gong [76], stress events caused by earthquakes are those of low-cycle fatigue. Investigations of GRs and ECRs are deficient. The reason could be that galvanized coating and epoxy coating rarely participate in the mechanical properties of reinforcements. Current investigations of fatigue in SCRs and SFCBs are shown in Table 3. The failure mode of tubby SFCBs is fiber fracture with fiber split, while that of slender SFCBs is mainly fiber split. More energy is dissipated in the tensile zone than in the compression zone, corresponding to the anisotropy of SFCBs. Bidirectional degradation effect is found after initial fiber failure. The fatigue performance of SFCBs is dominated by the fiber layer [75,77]. Yang et al. [78] studied the fatigue performance of ballastless track slabs subjected to different fatigue loading. Their results showed that after 3,000,000 fatigue cycles, the crack width of the SFCB slab was only 0.15 mm. At higher load levels, the traditional RC slab was close to fracture, while the stiffness of SFCB only reduced by 6%.
In terms of SCRs, the failure mode of SCRs in fatigue is buckling, and the buckling deformation is more apparent with increase in the strain amplitude. The energy dissipations in compression and tension zones are approximately equal, which corresponds to the isotropy of steel. The fatigue performance of the SCR was close to the BSR in [69,79,80]. Besides seismic performance, fire-resistance is also an important criterion in construction [81]. The basic post-fire mechanical properties of reinforcements have been widely investigated [74,82,83,84,85,86,87], but there are scarce resources for post-fire low-cycle fatigue properties [88,89]. Hua et al. [90,91] tested the low-cycle fatigue properties of SCRs with different elevated temperatures and cooling methods. Specifically, the SCR kept metallurgically bonding after fatigue or post-fire fatigue. The elevated temperature could cause a reduction in the number of cycles leading to fatigue. When the temperature was above 800 °C, the energy dissipation per cycle experienced a dramatic drop, which indicated that the elasticity of the SCR suddenly decreased. Temperature had little effect on the hysteresis curves for SCR subjected to cooling in air, but the curves of SCR subjected to cooling in water became slender when temperature exceeded 700 °C.
Table 3. Experiments on fatigue properties.
Table 3. Experiments on fatigue properties.
RefTypeVariableRemarks
Sun et al., 2017 [75]BSR/
SFCB
Bar typePolymers 14 04782 i005
Li et al., 2022 [69]SCRDiameter, strain rate, strain amplitudePolymers 14 04782 i006
Hua et al., 2022 [79]SCRStrain amplitudesPolymers 14 04782 i007
Wang et al., 2022 [80]SCRSlenderness ratio, fatigue strainPolymers 14 04782 i008
Hua et al., 2022 [92]SCRfatigue damagePolymers 14 04782 i009
Hua et al., 2021 [90]SCRExposure temperaturePolymers 14 04782 i010
25 °C
Polymers 14 04782 i011
900 °C
Polymers 14 04782 i012
25 °C
Polymers 14 04782 i013
900 °C
Hua et al., 2022 [91]SCRExposure temperature, cooling methodPolymers 14 04782 i014
700 °C and CIW
Polymers 14 04782 i015
700 °C and CIA
Polymers 14 04782 i016
CIW
Polymers 14 04782 i017
CIA
Note: stainless cladding reinforcement (SCR); steel-FRP composite bar (SFCB); cooling in water (CIW); cooling in air (CIA).

3.3. Bond Strength

As the baseline, the bond strengths of steel bars have been commonly tested [93,94,95,96]. Long et al. [93] concluded that shallow embedment length was a cause of pull-out failure, where the load–displacement curve had a hump and nearly constant residual force. In this situation, the specimen failed before steel yielding. Increasing the embedment length could reduce the hazard of slipping failure, where the load–displacement curve showed strength development in the post-yield stage. Furthermore, with increase in loading rate, bond strength developed. The reason for this could be that radial cracks were limited to propagating to concrete by a higher loading rate.
Certain investigators have reported a reduction of bond strength by using GRs [27,95,97,98]. These experiments included pull-out, beam, and beam to column. The bond strength of GRs to concrete experienced a reduction of 4 to 17%. Pokorný [95] attributed the drop in bond strength to oxidizing zinc and hydrogen formation. However, in a beam end test, Kayali [96] reported that the bond strength of GRs fairly equaled steel bars, and further surface treatment was not necessary for the GR. Patnaik [27] proposed the pull-out test for BSRs and GRs. According to Patnaik’s results, the GR showed higher bond strength than the BSR, with 17% enhancement.
Many recent studies [27,31,96,99,100] have shown that ECR is deficient in bond strength, with the reduction varying from 5 to 35%. A larger decrease in bond strength was observed in beam tests in [31,99,100] than in pull-out tests in [27,96]. ECR reinforced concrete not only has lower bond strength, but the slipping distance at the same bond stress is also larger than that of uncoated bar reinforced concrete. Hasan et al. [31] pointed out that the concrete cover to the bar diameter ratio and the rib bearing area ratio were explicitly associated with bond strength. In beam tests, the thick concrete cover and strong rib indicated better bond performance. Furthermore, Assaad and Issa [100] concluded that the adhesion loss and relatively smooth surface of epoxy coating could be the cause of the decrease in bond strength.
There is a renewal of bond strength between SCRs and sea-sand concrete [101,102]. As concluded by Hua et al. [101], there was no obvious damage to SCRs after specimen failure. The specimens with longer concrete age had better bond performance. Increasing the concrete cover thickness to bar diameter ratio and adding polyoxymethylene fiber could strengthen the bond between SCRs with sea-sand concrete.
Although SFCBs improve the mechanical behavior of FRP bars, the bond strength of SFCBs still needs to be developed [94]. Surface-threaded treatment could develop the bond performance of SFCBs [94]. Similar to the failure mode of ribbed BSRs, surface-threaded SFCBs experience splitting failure, which indicates that the stress can properly transfer to concrete. The application of a sand coat was regarded as a method to develop the bond strength of FRP bars by increasing surface roughness. The bond strength of sand-coated SFCBs were enhanced to a maximum of 50% over that of SFCBs without a sand coating [62].
Table 4 summarizes the bond strength tests for BSRs, ECRs, GRs, and SFCBs. The retention is defined as the bond strength of anti-corrosion reinforcement divided by the bond strength of BSRs. Specifically, most of the tests indicate that existing coat technologies have drawbacks in relation to bond strength. Apart from the effects of cover thickness and bar diameter, the reasons for reduction of bond strength can include the following: low stiffness, poor toughness, adhesion loss between the coat and bar, and deficient strength of the rib. Surface threading and sand coating can improve the bond performance of SFCBs, but brittle failures occurred in sand-coated GFRP specimens in pull-out tests in [62]. Figure 5 shows examples of failure performance. Specifically, the ribs of ECRs are worn-out after pull-out progress, while the resin surface of SFCBs is also scratched. In contrast, SCRs shear off the concrete between ribs. This diversity is caused by different strengths of coating. Figure 6 compares the bond strengths and bond strength retentions of anti-corrosion reinforcements. The bond strength of anti-corrosion reinforcements is distributed in the range from 3.21 to 20.9Mpa. The GR, ECR, and SFCB show deficient bond strength retention at lower bounds. Nevertheless, the bond strength retention of ECRs is still less than 100% at the upper bound. The diversity of bond strength retention reflects the contradiction of GRs investigations but proves the shortage of ECRs. The bond strength of SCRs is close to that of BSRs at the upper and lower bounds. This indicates that the performance of bond strength in SCRs is similar to BSRs. The SFCB satisfies bond strength at the upper bond because it adopts the surface-threaded and sand-coated techniques.
Table 4. Experiments on bond strength.
Table 4. Experiments on bond strength.
BarTestBond Strength (MPa)Retention % Ref.
BSRPull-out 18.8~22.6-[93]
BSRBeams 3.34~3.84-[95]
BSRBeam end13.2-[96]
BSRPull-out 12.9-[94]
ECRPull-out-93[27]
ECRBeams-65~85[99]
ECRBeams -59~95[31]
ECRPull-out8.7~15.881~89[100]
ECRBeam end 9.0~9.968~75[96]
GR Pull-out-117[27]
GRBeams 3.21~3.6194~96[95]
GRBeam-column-83~94[97]
GRBeam end 13.5102[96]
GRPull-out13.187[98]
SCRPull-out4.17~18.19-[101]
SCRPull-out9.4~16.591~95[102]
SFCBPull-out6.1~13.546~102[94]
SFCBPull-out11.6~15.5-[62]
SFCBPull-out20.1~20.997~101[39]
SFCBPull-out11.0~20.965[103]
SFCBPull-out11.8~16.959~95[104]
Note: black steel reinforcement (BSR); galvanized reinforcement (GR); epoxy coated reinforcement (ECR); stainless cladding reinforcement (SCR); steel-FRP composite bar (SFCB).
Figure 5. Failure performances of (a) ECR [105], (b) SFCB [94], (c) SCR in the bond test [101].
Figure 5. Failure performances of (a) ECR [105], (b) SFCB [94], (c) SCR in the bond test [101].
Polymers 14 04782 g005
Figure 6. Bond strengths and bond strength retentions due to corrosion [39,94,95,96,98,102].
Figure 6. Bond strengths and bond strength retentions due to corrosion [39,94,95,96,98,102].
Polymers 14 04782 g006

4. Behavior after Corrosion

4.1. Corrosion Mechanism

The corrosion mechanism can be classified according to material types, namely metal and nonmetal. For metal materials, oxidation is a common challenge. The metal can generate a passive film to prevent corrosion. The passive layer of black steel reinforcements (BSRs) is a submicroscopic γ -Fe2O3 film [12,106]. However, it can be attacked by Cl [8,106,107,108]. The chloride ions can replace the oxygen ions [106,107,108], and the insoluble oxide is, thus, transmuted to soluble chlorine salt. After the passive film is damaged, the steel bar is electrochemically corroded. As shown in Figure 7a, the cathodic and anodic reactions occur simultaneously at the surface of BSRs where the steel matrix transfers the ions [8,109]. The iron atoms lose electrons to the anode. The ferrous ions combine with free hydroxide ions, which produces ferrous hydroxide. The ferrous hydroxide is further oxidized to ferric oxide, generally called rust [109]. In consequence, rust that is 2–10 larger than the passive product gathers on bars, which expands the concrete by a pressure of 3–4 MPa [16]. A crack thereby propagates from the bars to the surface of the concrete. In terms of galvanized reinforcements (GRs) and stainless cladding reinforcements (SCRs), either zinc or stainless steel can generate a more stable passive film than steel, which are Zn-based and Cr-based oxides, respectively. The galvanized coat can provide extra protection as the sacrificed coat [110]. As shown in Figure 7c, in the case of the steel partly exposed to an aggressive environment, the zinc loses electrons instead of the iron. The oxidation of zinc is dense and steady, and further corrosion can be prevented [8,111]. For SCRs, the corrosion mechanism of stainless steel is a complex subject that is worth research driven by practical significance. Pit corrosion is the important mechanism in stainless reinforcement in the marine environment. As shown in Figure 7e, the mechanism of pitting corrosion is a negative feedback loop of local acidification [112]. Apart from chemical corrosion, corrosion under sustained stress is also worth investigating when stainless steel is adopted as the reinforcement [113,114]. The elastic modulus of most stainless steel is around 200 GPa, but the elastic modulus of Cr2O3 is 280 GPa at 25 ℃ [115]. Due to this difference, the passive film can physically rupture when deformation occurs. In terms of non-metal material, moisture is the cause of degradation. For example, as an organic material, epoxy has certain permeability which allows the passage of corrosion substances [110,116]. Once enough corrosion products accumulate on the surface of steel, disbondment is accelerated because of the expansion stress from rust and blisters [110,116]. The schematic of under-film corrosion is shown in Figure 7b [30]. As a recent research hot spot, graphene oxide nanocomposite was found effective in improving the corrosion resistance of epoxy coating, as shown in Figure 3 [117,118,119,120]. The FRP (Fiber Reinforced Polymer) coat principally accounts for the corrosion resistance of SFCBs [38]. FRPs can be decomposed by strong alkaline conditions in a wet environment, which is the basis of hydrolysis [40,121,122,123,124]. As shown in Figure 7d, the fiber and resin de-bond in hydrolysis. Subjected to sustained load, corrosion channels appear and promote moisture diffusion. These damages shorten creep rupture time [40,123,124]. The chloride threshold is the concentration of chloride on the surface of reinforcement required to decompose the passive layer [125,126,127]. It is one of the parameters to describe the corrosion resistance of reinforcements. The second Strategic Highway Research Program (SHRP2) summarized the chloride threshold for various reinforcement steel types. The average chloride threshold of BSRs was 0.68; while the average chloride thresholds of GRs, ECRs, and SCRs were1.27, 0.63, and 5.2 [125]. The chloride threshold of SFCBs was not reported. ECRs have a lower average chloride threshold than BSRs, attributed to it being difficult to avoid the coating defect in the field.
Figure 7. Corrosion mechanism of the (a) BSR, (b) ECR, (c) GR, (d) FRP bar, (e) Stainless reinforcement [2,30,111,123,128].
Figure 7. Corrosion mechanism of the (a) BSR, (b) ECR, (c) GR, (d) FRP bar, (e) Stainless reinforcement [2,30,111,123,128].
Polymers 14 04782 g007

4.2. Tensile Strength

In terms of the mechanical properties of steel bars after corrosion, a large number of experiments have been conducted [106,129,130,131]. Xu et al. [129] reported that the yield plateau was observed to shorten and even disappear when the mass loss was more than 2%. As reported by C.A. Apostolopoulos et al. [130,132], both effective and apparent strength decreased with an increase in exposed days, but apparent strength experienced a more dramatic drop. Almusallam [106] also concluded that the elongation showed distinct degradation with corrosion. Zhang et al. [131] reported that the ultimate strength closed to yield strength with aggravating corrosion, which implied a higher risk of brittle failure.
Investigations into the mechanical properties of coated bars after corrosion have been more recent [33,39,70,133,134]. Ismail and Muhammad [70] tested the tensile behavior of corroded GRs. The zinc was depleted in corrosion, but the yield strength, ultimate strength, and elongation to fracture were observed to develop after immersion. Miyazato and Nakazawa [135] experimented on the tensile performance of ECR corresponding to varying damage areas. Their results showed that tensile strength was basically maintained under a chloride environment. Gao [133] tested the mechanical behavior of SFCBs subjected to corrosion and sustained load. The ultimate strength of SFCBs was observed to decrease after immersion, with strength retention of 88.84%. Ge et al. [39] presented a similar test and found the maximum strength retention was 87.27%. Zhou et al. [136] polarized the CFRP bar and SFCB to assess the feasibility of the bars with impressed current cathodic protection (ICCP). In the result, based on the prediction model, the service life of the CFRP bar was 62 years, while that of SFCB was only 7 years. The reason was that the inner steel of SFCB corrodes much faster than the resin of CFRP. Zhou et al. [137] reported the corrosion rate of carbon-type SFCB was less than 1/10 of BSR, and that of glass-type SFCB was less than 1/100 of BSR. Hua et al. conducted electrochemical accelerated corrosion tests for SCRs [33,134,138] and reported that both apparent yield strength and ultimate strength of SCRs decreased after corrosion, but the reduction of yield strength was less than that of BSR. They also proposed predictive equations and a stress–strain model to clarify the corrosion performances and mechanical properties of artificially damaged SCRs with different corrosion ratios.
Table 5 summarizes the experiments on the tensile behavior of corroded bars. The experimental results generally concern retention of yield strength, ultimate strength, and elongation to fracture. A part of the investigation compares the results to current specifications. Specifically, BSRs have been widely studied [106,129,130] and the common drawback reported is the rapid degradation of elongation to fracture in BSRs under corrosion. In terms of GRs and ECRs, there are scarce investigations on tensile strength. The decomposition of the galvanized layer has a negligible effect on the tensile strength of reinforcement [70]. The degradation of SFCBs is generally expressed as a reduction of maximum strength [39,133]. After corrosion, SCRs also show degradation of ductility, but the degree of degradation is lower than for BSRs [33,134]. Figure 8 compares the partial tensile behaviors of BSRs, GRs, SFCBs, and SCRs. Subjected to NaCl solution, the coatings of GRs and SFCBs corroded, but the steel substrate was effectively protected. The tensile behaviors of corroded specimens, thereby, had no obvious changes to the uncorroded specimens [39,70,133]. The corroded tensile behaviors of BSRs is expressed as embrittlement [106,130,131,132]. The yield plateau of BSRs disappears when the corrosion degree reaches 12.6% [106]. However, for SCRs, necking is still observed even when the corrosion degree reaches 20% [33]. This could be evidence that the degradation of SCRs is slower than that of BSRs under corrosion.
Table 5. Accelerating tests of uncoated bars and coated reinforcements.
Table 5. Accelerating tests of uncoated bars and coated reinforcements.
Ref.Type ConditionsSolutionRemarks
Almusallam 2001 [106]BSRElectronic corrosion in concrete 5% NaCl Proved that the elongation has a distinct degradation with corrosion.
Ismail 1997 [70]GRSalt solution bath in concrete5% NaCl Found that the tensile properties are improved after immersion.
Miyazato [135]ECRElectronic corrosionChloride environmentFound that the speed of corrosion correlates to the damage area of ECR.
Gao 2020 [133]SFCBSolution bath with sustained stress 3.5, 7.0% NaClFound that the ultimate tensile strength is degraded.
Zhou et al., 2020 [136]SFCBElectronic corrosionSeawaterFound that compared with CFRP, the deterioration of SFCB is serious due to the corrosion of the inner steel.
Ge et al., 2021 [39]SFCBSolution bath with sustained stress 3.5, 7.0% NaClProved that the sustained stress amplifies the degradation.
Hua et al., 2021 [33]SCRElectronic corrosion5% NaClFound that the corrosion has a negligible effect on yield strain.
Hua et al., 2021 [134]SCRElectronic corrosion5% NaClFound that the εu and εuy decrease with intensifying the corrosion.
Hua et al., 2021 [138]SCRElectronic corrosion5% NaClFound that the increase of corrosion ratio led to the decrease of fy, fu, εu and δ, and under the same corrosion ratio, the fy and fu of corroded BSRs increased with the increase of W/D.
Note: black steel reinforcement (BSR); galvanized reinforcement (GR); stainless cladding reinforcement (SCR); steel-FRP composite bar (SFCB).
Figure 8. Tensile behaviors of BSR [106], GR [70], SFCB [39], and SCR [33] after corrosion.
Figure 8. Tensile behaviors of BSR [106], GR [70], SFCB [39], and SCR [33] after corrosion.
Polymers 14 04782 g008

4.3. Fatigue Properties

Hasegawa et al. [54] discussed the effect of humidity on the corrosion fatigue mechanism of galvanized AISI 1045 steel. In the low cycle fatigue region, the fatigue strength of galvanized specimens showed no obvious difference with change in humidity. However, a reduction of fatigue strength due to galvanization was reported when the number of cycles to failure was larger than 104. Hua et al. [134,139] investigated the corroded low-cycle fatigue performance of SCRs. SCRs were electronically corroded to a controlled degree. The corrosion initialized at the surface of SCRs and gradually deepened. With increase of corrosion degree and fatigue strain amplitude, the cycles of fatigue and total energy dissipation reduced. The above investigations are compared in Table 6. Both reinforcements show ductile fractures in the low-cycle region. There are gaps in the interface of the galvanized layer and steel core, a separation that was also observed in the SCR when the strain amplitude increased [139].
So far, a deficiency of investigations in corroded tensile and fatigue properties of ECRs has been found. The basic reason is that the steel substrate dominates the tensile and fatigue properties of ECRs. Even when considering corrosion, researchers prefer to investigate corrosion resistance based on individual electrochemical theories or by experiments on individual components, but mechanical tests are not involved [140,141,142,143,144,145].

4.4. Bond Strength

Corroded bond strength is a major area of interest within the field of coated reinforcement. The coat is commonly expected to improve the bond performance of reinforcement to concrete in an aggressive environment. In cases of galvanized coating, Pokorný et al. [2] pointed out that degradation of bond strength in GR reinforced concrete was mitigated. The evidence for this was found in research [146,147]. According to the results presented, the bond strength of galvanized specimens was usually less than that of black steel specimens without corrosion. However, after accelerating tests, this difference was almost eliminated, and the bond strength of galvanized specimens was even beyond that of the black steel specimens. Accumulation of hydrogen and decomposition of the zinc layer could be the reasons for the degradation of bond strength. As shown in Figure 9a, hydrogen gas is generated at the interface and increases porosity [2].
Similarly, epoxy coats can also develop bond strength between concrete and reinforcement during corrosion [148]. El-Hawary [149] set specimens in tanks of seawater. With increase in exposure time, the bond strengths of the BSR reinforced specimens decreased faster than those of the ECR reinforced specimens. As shown in Figure 10, after 18 months of exposure in the Gulf, the bond strength in ECR reinforced specimens climbed to 108% of the bond strength in uncoated bar reinforced specimens. This enhancement was attributed to salt crystallization in the concrete pores.
In terms of SFCBs, bond performance is different to that of previously coated reinforcement. The bond strength increases when SFCBs start to be exposed to an aggressive environment, then decreases with exposure time [38,39,150]. The swelling effect of FRPs in a wet environment could be a cause of the enhanced bond strength, which the corrosion degradation counteracts, exceeding the swelling effect, as shown in Figure 9b [150].
As shown in Figure 10, the bond strength of SFCB reinforced specimens is not sensitive to an exposed environment. Failure performances are similar before and after corrosion, comparing Figure 5c to Figure 7b. The enhancement of bond strength is ascribed to the swelling effect of the outer FRP in a water environment. In contrast, the bond strength of uncoated bar reinforced specimens increases at first because the corrosion products roughen the surface of the bar. Then, the bond strength drops due to the expansion stress of rust. Furthermore, SFCBs are reported to suffer more severe corrosion in conditions of continuous immersion, compared to a wet–dry cycling environment, while BSRs are the opposite [150].
Table 7 summarizes the tests of bond strength with corrosion, where retention is defined as the bond strength of coated bar reinforced specimens divided by bond strength of BSR reinforced specimens. Specifically, galvanized technology develops the bond strength of reinforcement and concrete with corrosion [27,146,147]. The epoxy coat is effective when exposed to an ocean environment [149]. The bond strength of SFCB reinforced concrete is controversial. It has good performance in a wet–dry environment [150]. However, corrosion may be severe when the specimens are continuously immersed in salt solution or seawater [39,150]. Further investigations are necessary.
Combining Table 7 with Table 5 it can be deduced that acceleration tests usually simulate the aggressive environment by electrochemical corrosion, solution immersion, salt spray, and wet–dry cycle, and the relevant solutions include artificial seawater, natural seawater, 3.5% NaCl, corresponding to the marine environment, or 5%NaCl, corresponding to concrete pore fluid. The corrosion set depends on the experimental objectives and the corrosion resistance of reinforcements. For example, electrochemical corrosion was found in experiments interested in mechanical behaviors of metal reinforcements in varying corrosion degrees. Indeed, these experiments usually consider intensive corrosion. In contrast, non-electrochemical corrosion can be used in metal and nonmetal reinforcements, and the experiments also try to quantify the corroded performance of reinforcements on a time scale. In the anti-corrosion reinforcements that were reviewed, the experiments on GRs and ECRs included electrochemical and non-electrochemical corrosion. SFCBs were experimentally corroded by solution because their corrosion mechanism is close to that of FRPs. SCRs are only electrochemically corroded in experiments because it is difficult to simulate a corrosive solution for the concrete or natural environment that corrodes SCRs in an acceptable time frame.
Table 7. Experiments on bond strength after corrosion.
Table 7. Experiments on bond strength after corrosion.
Bar TestCondition Solution PeriodRetention % Ref.
GRPull-outElectrochemical corrosion pH 12
3.5% NaCl
6, 14, 18 days105~115[146]
GRPull-outElectrochemical corrosion5% NaCl10 days120[27]
GRBeamHalf immersionArtificial seawater
natural seawater
1, 12, 24, 60, 120 months.73~120[147]
ECR Pull-outElectrochemical corrosion 5% NaCl10 days87[27]
ECRPull-outHalf immersionSeawater0, 6, 12,18 months84~108[149]
SFCBPull-outSolution bath with sustained stress 3.5, 7.0% NaCl 45, 90, 135 days.85~102[39]
SFCBPull-out;
Beam
Wet–dry cyclesArtificial seawater30, 60, 90 days.78~86[38]
SFCBPull-outWet–dry cyclesArtificial seawater30, 60, 90 days.91~135[150]
SFCBPull-outWet–dry cyclesArtificial seawater3, 6, 9 months74~99[151]
Note: galvanized reinforcement (GR); epoxy coated reinforcement (ECR); steel-FRP composite bar (SFCB).
Figure 9. Failure performance of (a) GR and (b) SFCB in the pull-out test [2,38].
Figure 9. Failure performance of (a) GR and (b) SFCB in the pull-out test [2,38].
Polymers 14 04782 g009
Figure 10. Bond strengths and retentions of uncoated and coated reinforcement exposed to varying environments [38,147,149].
Figure 10. Bond strengths and retentions of uncoated and coated reinforcement exposed to varying environments [38,147,149].
Polymers 14 04782 g010

5. Applications

Over the past century, there has been an increase in the use of galvanized steel as a reinforcing material [27]. In the 1930s, civil construction in the USA regularly used GRs. In the 1950s, GRs started to be applied to bridge decks, which require strict crack control [27]. Yeomans [16] recorded field studies on galvanized steel reinforced bridges built from 1968 to 1979 in the USA and UK. The studies indicated that the galvanized coat offered effective protection for 15 to 18 years after the bridge was built. In terms of epoxy coated reinforcement, the application in bridges can be traced back to 1973 [27]. Epoxy coating was used to reinforce the substructures of a segmental bridge in the Florida Keys, USA. Since the 1970s, ECR has been widely used in bridges in the USA. However, certain field studies at the end of the 1990s reported that the epoxy coat lost efficiency in protecting steel from corrosion after 15 to 22 years of service [3,28]. The application of SCRs was mainly concentrated in the early 21st century [42,43].
In terms of cost, the galvanizing bar is twice as expensive as the steel bar [72], which could cause up to 50% extra initial construction costs, depending on the region [16]. GRs shows cost-effectiveness in life cycle analysis, compared to BSRs [53]. However, repair is still necessary because the durability of galvanizing reinforcement has not yet met the requirements of a 100-year design lifetime [8]. The effective protection period of the epoxy coat may be less than the 50-year design lifetime time of the civil structure [3]. Therefore, maintenance must always be considered. For an example of life cycle analysis [17], the construction cost of using ECRs only involves a 20% increase because the price of epoxy coating reinforcement is 1.3 times that of BSRs [72]. However, patching and repair continuously adjust the net present value such that the ECR proposal is not competitive in the final comparison.
A considerable discount is brought by stainless cladding technology. Basham [72] indicates that the unit cost of SCRs is 2.5 times that of BSRs, which is much more economical compared to the stainless bar [152]. Indeed, stainless steel is six to nine times more expensive than carbon steel [73]. Construction using SCRs is regarded as requiring no maintenance in a 100-year design lifetime [60,73,153].
Table 8 summarizes the applications of coated reinforcement, some images are shown in Figure 11. The data was collected from papers, company websites, and news. In general, most scenarios of using anti-corrosion reinforcement were marine infrastructures that require strict serviceability and have expensive maintenance costs. As demonstrated in Figure 12, the development of applications of GRs, ECRs, and SCRs is imbalanced in regions and time. There are considerable projects using anti-corrosion reinforcements in North America, but they are hard to find in Africa. Anti-corrosion reinforcements experienced a dramatic increase from 1990 to 2010. During this period, most projects were still built in North America, but Asian, European, and South American engineers also adopted anti-corrosion reinforcements. The development of society may affect the applications of anti-corrosion reinforcements. GRs have the earliest applications, followed by ECRs and SCRs. GRs have steadily increased in projects using anti-corrosion reinforcements. ECRs jumped fast after 1900, and their applications exceeded GRs after 1990. The mature manufacture and low cost of ECRs has promote their application. The number of projects using SCRs has remained approximately flat after the first increase from 1900 to 2010. Indeed, compared to GRs and ECRs, the relatively immature manufacture and high costs limit the popularity of SCRs. In 2015, the stainless-clad bimetallic steel bar (SCBSB) was produced by Hunan 3T New Materials CO., LTD [60]. The SCBSB improves the mechanical properties of SCRs and reduces the cost by approximately 30% [36,37,60,62,63,90,139]. A bay bridge in China adopted SCBSBs in 2021 [154]. As a relatively new material, the practical engineering application of SFCBs is rare.
Table 8. Application of coated reinforcements.
Table 8. Application of coated reinforcements.
Reinforcement Project Year Ref.Figure
GRThe Longbird Bridge, Bermuda1953[155]
GRThe Royal Bermuda Yacht Club, Bermuda1968[16]
GRThe Egg, Albany, USA1978[155]
GRThe new Watford Bridge, Bermuda, USA1979[16]
GRSewerage outfall tunnels, Australia-[16]Figure 11a
GRAthens Bridge, Pennsylvania, USA1953[16]
GRTioga Bridge, Pennsylvania, USA1964[16]
GRB776 pedestrian bridge, South Africa1964[155]
GROminichi Pier, Japan-[16]
GRLibrary Tower, Sydney, Australia-[16]
GRDeep Tunnel Sewage System, Singapore-[155]
GRSydney Opera House, Sydney, Australia1975[155]Figure 11b
GRParliament House, Australia1983[155]
GRRome Mosque, Italy1995[155]
GRSept-Ile Multi-Purpose Wharf Complex, Canada2014[155]
ECR Segmental bridge substructures in the Florida Keys, USA 1973[28]
ECR Bridge decks located in Virginia, Wisconsin, Pennsylvania, New York, and Ohio, USA1981[28]
ECRSchieβberg Road Bridge in Leverkusen, Germany1988[156]
ECR12 km-long Belt Tunnel between Sprogø and Zealand in Denmark1996[56]
ECRShantou LPG Wharf Engineering, China1997[157]
ECRBachimen Bridge, China2000[158]
ECRMinistry of Defense building in Riyadh, Saudi Arabia2003[56]
ECRThe Woodrow Wilson Bridge, Alexandria, USA2006[29]
ECRMuseum of Islamic Art in Doha, USA2008[56]
ECRAlpha and Bravo Wharf Improvements (Marinas), Polaris Point, Guam2008[159]
ECRRichmond Olympic Speed Skating Oval, Canada2008[159]
ECRThe Biggs Rapids/Sam Hill Bridge, USA2009[159]Figure 11c
ECRBandra Worli Sea Link. India 2009[29]
ECRUS embassy in the Philippines, USA2012[56]
ECRShijiazhuang–Wuhan passenger railway station in Henan, China2012[56]
ECR11th Street Bridge, Washington, USA2013[159]
ECRI-90 Dresbach Bridge Replacement2016[159]Figure 11d
SCRThree lane bridges, R12-4 of 33045, Lansing, Michigan, USA.2001[42]
SCRThe bridge in I-94, Berrien County, Michigan, USA.2008[42]
SCRHighway 9 over South Holland canal—Ontario2000[43]
SCRAshland avenue bridge—Brown County, Green Bay, Wisconsin2001[43]Figure 11e
SCRHydro-Electric Power Station in Nant, Scotland—UK2002[43]Figure 11f
SCRSturgeon River, Alberta2002[43]
SCRWest Valley City interchange—East Bound, West Fargo, North Dakota2001[43]
SCRPutnam Road bridge, Shenectady County, N.Y.S.2001[43]
SCRSpan A of B 635 of Route 460 in Campbell County, Virginia2002[43]
Note: galvanized reinforcement (GR); epoxy coated reinforcement (ECR); stainless cladding reinforcement (SCR).
Figure 11. Applications of coated reinforcements: (a) Sewerage outfall tunnels, (b) Sydney Opera House, (c) The Biggs Rapids/Sam Hill Bridge (d) I-90 Dresbach Bridge Replacement (e) Ashland Avenue Bridge, (f) Hydro-Electric Power Station [16,43,155,159].
Figure 11. Applications of coated reinforcements: (a) Sewerage outfall tunnels, (b) Sydney Opera House, (c) The Biggs Rapids/Sam Hill Bridge (d) I-90 Dresbach Bridge Replacement (e) Ashland Avenue Bridge, (f) Hydro-Electric Power Station [16,43,155,159].
Polymers 14 04782 g011aPolymers 14 04782 g011b
Figure 12. Applications of GR, ECR, SCR corresponding to the region and time Note: galvanized reinforcement (GR); epoxy coated reinforcement (ECR); stainless cladding reinforcement (SCR); Asia (AS); Europe (EU); North America (NA); South America (SA); Oceania (OA); Africa (AF).
Figure 12. Applications of GR, ECR, SCR corresponding to the region and time Note: galvanized reinforcement (GR); epoxy coated reinforcement (ECR); stainless cladding reinforcement (SCR); Asia (AS); Europe (EU); North America (NA); South America (SA); Oceania (OA); Africa (AF).
Polymers 14 04782 g012

6. Future Works and Recommendations

Based on this review of previous studies and applications, recommended future research follows:
  • Since GRs have been applied to constructions for many years, further studies are recommended to combine laboratory tests and field studies. This would help in precisely understanding the behaviors of GRs in concrete.
  • ECRs have an inherent problem of permeability, which correlates to failure in corrosion resistance, as reported in early field studies. The corrosion performance of structures using ECRs needs continuous attention. Based on bibliometric analysis, this review finds that graphene oxide nanocomposite could improve the corrosion resistance of epoxy and enhance the performance of ECRs. This could be a possible research area.
  • The corrosion mechanism of SCRs in concrete is a complicated subject. Current investigations study the corrosion behavior of SCRs by electrochemical corrosion. This is feasible but still different from the corrosion behavior of SCRs in concrete. Thus, more proper accelerated conditions need to be researched. In addition, investigation of the corroded bond strength of SCRs is rare, and future studies should fill this gap.
  • The corrosion mechanism of SFCBs has not yet been individually investigated and the corrosion model of SFCBs in concrete is worth studying.
  • Anti-corrosion reinforcements are used in infrastructures that may experience extreme loadings, such as fire, earthquake, storm and so on. Further experiments are recommended to couple corrosion with more loading scenarios.
  • Anti-corrosion reinforcements are designed to meet requirements for the long-term use of infrastructures in an aggressive environment, which makes it necessary to conduct cost–benefit analysis. Thus, life-cycle cost analysis of structures using anti-corrosion reinforcements should be focused on.

7. Conclusions

This paper summarizes the existing knowledge on anti-corrosion reinforcements incorporating galvanized reinforcements (GRs), epoxy coated reinforcements (ECRs), stainless cladding reinforcements (SCRs), and steel-FRP composite bars (SFCBs) by providing a comprehensive review. The key aspects include manufacture, behaviors without corrosion, corrosion mechanism, and behaviors after corrosion. According to the presented investigations, the conclusions and research needs are drawn as follows:
Influence of Manufacture
  • The heating process of producing GRs and ECRs can reduce their ductility, especially for coating cold-twisted steel bars.
  • The rolling temperature may affect the strength of SCRs. With increase in rolling temperature, the promotion of strength is more distinct.
  • The winding process has a negligible effect on the mechanical properties of SFCBs.
  • GRs and ECRs should focus on minimizing the negative effect of manufacture on performance; while SCRs and SFCBs should reduce the cost and increase the production capacity.
Behaviors without Corrosion
  • The tensile and fatigue behaviors of GRs and ECRs are mainly dominated by the steel substrate. They are expected to be as applicable to most projects as ordinary reinforcement.
  • The tensile and fatigue behaviors of SCRs and SFCBs depend on the coating and core, and their interaction. SCRs show similar behaviors to BSRs because stainless steel and black steel have similar mechanical properties while they are metallurgically bonded, even after failure. SFCBs couple elastic–plastic steel and linear elastic FRP, which provides stable secondary stiffness. The force transfers between coating and core by friction.
  • The bond strength of ECR and GR reinforced concrete was reported to be deficient. The performance of SCRs regarding bond strength is similar to that of BSRs. After surface treatment, SFCBs could have better performance than BSRs.
Corrosion Mechanism
  • Due to cathodic protection, corrosion first consumes the galvanized layer and then the steel substrate.
  • The steel substrate of ECR is usually first corroded because corrosive materials prefer to permeate the epoxy instead of decomposing.
  • The corrosion of SCRs is complicate, combining electrochemistry with physics, and further research is needed.
  • SFCBs have a similar corrosion mechanism to that of FRP bars, in which hydrolysis and sustained load can simultaneously contribute to the degradation of resin and fibers.
Behaviors after Corrosion
  • Corrosion in galvanized layers has a negligible effect on the tensile and fatigue properties of GRs.
  • SCRs have lower degradation of ductility in a given degree of corrosion compared to BSRs.
  • The steel substrate of SFCBs was not corroded, and the degradation of SFCBs in corrosion is in ultimate strength instead of ductility.
  • The fatigue properties of corroded SCRs are similar to those of corroded BSRs.
  • GRs, ECRs, and SFCBs ensure better performance regarding bond strength than BSRs after corrosion.
Applications of Anti-Corrosion Reinforcements
  • The advanced use of anti-corrosion reinforcements is uneven in regions, and may correlate to the development of technology and the economy.
  • GRs and ECRs have considerable applications worldwide. With developments in their manufacture, SCRs may be an economical alternative to other anti-corrosion reinforcements. The application of SFCBs is rare.

Author Contributions

Conceptualization, L.Y., X.X. and N.W.; methodology, X.X. and W.D.; software, W.D.; investigation, L.Y., N.W. and W.D.; writing—original draft preparation, W.D.; writing—review and editing, L.Y. and N.W.; project administration, J.H. and Z.C.; funding acquisition, N.W. and L.Y. All authors have read and agreed to the published version of the manuscript.

Funding

This study was financially supported by the National Natural Science Foundation of China (Grant No. 52108115), the General Program of China Postdoctoral Science Foundation (2019M663442), Scientific and Technological Research Program of Chongqing Municipal Education Commission (KJQN202001216), Wanzhou District Science and Technology Innovation Project (20210306, Study on bearing mechanism and buried depth optimization of corrugated guardrail column of low-grade highway in mountainous area), and Cooperation projects between universities of Chongqing and institutes affiliated to the Chinese Academy of Sciences (HZ2021012).

Conflicts of Interest

The authors declare no conflict of interest.

Abbreviations

BSRblack steel reinforcement
GRgalvanized reinforcement
ECRepoxy coated reinforcement
SCRstainless cladding reinforcement
FRPfiber reinforced polymer
CFRPcarbon fiber reinforced polymer
GFRPglass fiber reinforced polymer
BFRPbasalt fiber reinforced polymer
SFCBsteel-FRP composite bar
SCBSBstainless-clad bimetallic steel bar

References

  1. Green, W.K. Steel reinforcement corrosion in concrete—An overview of some fundamentals. Corros. Eng. Sci. Technol. 2020, 55, 289–302. [Google Scholar] [CrossRef]
  2. Pokorný, P.; Tej, P.; Kouřil, M. Evaluation of the impact of corrosion of hot-dip galvanized reinforcement on bond strength with concrete—A review. Constr. Build. Mater. 2017, 132, 271–289. [Google Scholar] [CrossRef]
  3. Manning, D.G. Corrosion performance of epoxy-coated reinforcing steel: North American experience. Constr. Build. Mater. 1996, 10, 349–365. [Google Scholar] [CrossRef]
  4. ECi. A Global Need. Available online: https://corrosioninstrument.com/gn/ (accessed on 23 May 2022).
  5. ASCE Infrastructure Report Card. 2017. Available online: https://blog.envirosight.com/2017-asce-infrastructure-report-card (accessed on 31 October 2022).
  6. Hong, N. Economic loss and protection technology of reinforcement corrosion. In Proceedings of the 20th Anniversary of the Establishment of the Chinese Society for Corrosion and Protection and the 99th Academic Annual Meeting, Beijing, China, 7 November 1999; Available online: https://d.wanfangdata.com.cn/conference/99427 (accessed on 23 May 2022).
  7. Sika, B.T. Refurbishment Protective Coatings for Concrete Sika—Your Partner; Sika: Hong Kong, China, 2016. [Google Scholar]
  8. Zhao, B. Study on the Corrosion and Protection of the Coated Steel Rebar in Concrete; Xiamen University: Xiamen, China, 2007. [Google Scholar]
  9. Elnaggar, E.M.; Elsokkary, T.M.; Shohide, M.A.; El-Sabbagh, B.A.; Abdel-Gawwad, H.A. Surface protection of concrete by new protective coating. Constr. Build. Mater. 2019, 220, 245–252. [Google Scholar] [CrossRef]
  10. Diamanti, M.V.; Brenna, A.; Bolzoni, F.; Berra, M.; Pastore, T.; Ormellese, M. Effect of polymer modified cementitious coatings on water and chloride permeability in concrete. Constr. Build. Mater. 2013, 49, 720–728. [Google Scholar] [CrossRef]
  11. Goyal, A.; Ganjian, E.; Pouya, H.S.; Tyrer, M. Inhibitor efficiency of migratory corrosion inhibitors to reduce corrosion in reinforced concrete exposed to high chloride environment. Constr. Build. Mater. 2021, 303, 124461. [Google Scholar] [CrossRef]
  12. Pourbaix, M. Applications of electrochemistry in corrosion science and in practice. Corros. Sci. 1974, 14, 25–82. [Google Scholar] [CrossRef]
  13. Bolzoni, F.; Brenna, A.; Ormellese, M. Recent advances in the use of inhibitors to prevent chloride-induced corrosion in reinforced concrete. Cem. Concr. Res. 2022, 154, 106719. [Google Scholar] [CrossRef]
  14. Cheng, X.; Xia, J.; Wu, R.J.; Jin, W.L.; Pan, C.G. Optimisation of sacrificial anode cathodic protection system in chloride-contaminated reinforced concrete structure. J. Build. Eng. 2022, 45, 103515. [Google Scholar] [CrossRef]
  15. Wang, F.; Xu, J.; Xu, Y.; Jiang, L.; Ma, G. A comparative investigation on cathodic protections of three sacrificial anodes on chloride-contaminated reinforced concrete. Constr. Build. Mater. 2020, 246, 118476. [Google Scholar] [CrossRef]
  16. Yeomans, S.R. Galvanized Steel in Concrete: An Overview. In Galvanized Steel Reinforcement in Concrete; Elsevier: Amsterdam, The Netherlands, 2004; ISBN 978-0-08044-511-3. [Google Scholar] [CrossRef]
  17. Sajedi, S.; Huang, Q. Reliability-based life-cycle-cost comparison of different corrosion management strategies. Eng. Struct. 2019, 186, 52–63. [Google Scholar] [CrossRef]
  18. Wang, X.; Lin, Z. Robust, hydrophobic anti-corrosion coating prepared by PDMS modified epoxy composite with graphite nanoplatelets/nano-silica hybrid nanofillers. Surf. Coat. Technol. 2021, 421, 127440. [Google Scholar] [CrossRef]
  19. Stankiewicz, A.; Szczygieł, I.; Szczygieł, B. Self-healing coatings in anti-corrosion applications. J. Mater. Sci. 2013, 48, 8041–8051. [Google Scholar] [CrossRef] [Green Version]
  20. Zhang, R.; Yu, X.; Yang, Q.; Cui, G.; Li, Z. The role of graphene in anti-corrosion coatings: A review. Constr. Build. Mater. 2021, 294, 123613. [Google Scholar] [CrossRef]
  21. Idumah, C.I.; Obele, C.M.; Emmanuel, E.O.; Hassan, A. Recently Emerging Nanotechnological Advancements in Polymer Nanocomposite Coatings for Anti-Corrosion, Anti-Fouling and Self-Healing. Surf. Interfaces 2020, 21, 100734. [Google Scholar] [CrossRef]
  22. Li, Y.; Ning, C. Latest research progress of marine microbiological corrosion and bio-fouling, and new approaches of marine anti-corrosion and anti-fouling. Bioact. Mater. 2019, 4, 189–195. [Google Scholar] [CrossRef]
  23. Chen, C. Searching for intellectual turning points: Progressive knowledge domain visualization. Proc. Natl. Acad. Sci. USA 2004, 101, 5303–5310. [Google Scholar] [CrossRef] [Green Version]
  24. Chen, C. CiteSpace: Visualizing Trends and Patterns in Scientific Literature Outline What Can We Learn from Scientific; Nova Science Publishers: Hauppauge, NY, USA, 2015; pp. 1–21. [Google Scholar]
  25. Tang, M.; Hong, J.; Guo, S.; Liu, G.; Shen, G.Q. A bibliometric review of urban energy metabolism: Evolutionary trends and the application of network analytical methods. J. Clean. Prod. 2021, 279, 123403. [Google Scholar] [CrossRef]
  26. Chen, C. CiteSpace: A Practical Guide for Mapping Scientific Literature; Nova Science Publishers: Hauppauge, NY, USA, 2016; ISBN 978-1-53610-295-6. [Google Scholar]
  27. Patnaik, A.; Stroia, M.M. Structural and Corrosion Performance of Continuous Galvanized Rebar (CGR); GalvaBar: Catoosa, OK, USA, 2019. [Google Scholar]
  28. Zemajtis, J.; Weyers, R.E.; Sprinkel, M.M.; McKeel, W.T., Jr. Epoxy-Coated Reinforcement—A Historical Performance Review; Virginia Transportation Research Council: Charlottesville, VA, USA, 1996; p. 108. Available online: http://www.virginiadot.org/vtrc/main/online_reports/pdf/97-ir1.pdf (accessed on 27 May 2022).
  29. McDonald, D. Use and Performance of Epoxy-Coated Reinforcing Steel Over 37 Years. In Proceedings of the International Bridge Conference, Pittsburgh, PA, USA, January 2010; Available online: https://www.researchgate.net/publication/257121247_Use_and_Performance_of_Epoxy-Coated_Reinforcing_Steel_Over_37_Years (accessed on 31 October 2022).
  30. Kamde, D.K.; Pillai, R.G. Corrosion initiation mechanisms and service life estimation of concrete systems with fusion-bonded-epoxy (FBE) coated steel exposed to chlorides. Constr. Build. Mater. 2021, 277, 122314. [Google Scholar] [CrossRef]
  31. Halverson, A.D.; Bennett, J.E.; Clemena, G.G.; Hartt, W.H.; Jackson, D.R.; Moser, A.P.; Rosenberg, A.M.; Virmani, Y.P.; Kenneth, J.; Boedecker, J.; et al. Epoxy-Coated Reinforcement in Idghway Structures Preface. Transp. Res. Circ. Number 1993, 403, 5–16. [Google Scholar]
  32. Cross, W.; Duke, E.; Kellar, J.; Han, K.; Johnston, D. Stainless Steel Clad Rebar in Bridge Decks; South Dakota Department of Transportation: Rapid City, SD, USA, 2001; pp. 1–47. [Google Scholar]
  33. Hua, J.; Wang, F.; Huang, L.; Wang, N.; Xue, X. Experimental study on mechanical properties of corroded stainless-clad bimetallic steel bars. Constr. Build. Mater. 2021, 287, 123019. [Google Scholar] [CrossRef]
  34. Virmani, Y.P.; McDonald, D.B.; Pfeifer, D.W.; Sherman, M.R. Corrosion Evaluation of Epoxy-coated, Metallic-Clad and Solid metallic Reinforcing bars in Concrete. FHWA-RD-98; Federal Highway Administration: Washington, DC, USA, 1998; p. 137. [Google Scholar]
  35. Hurley, M.F.; Scully, J.R. Chloride threshold levels in clad 316L and Solid 316LN stainless steel rebar. In Proceedings of the CORROSION/2002 Annual Conference and Exposition, Denver, CO, USA, 7–11 April 2002. [Google Scholar]
  36. Wu, G.; Wu, Z.-S.; Luo, Y.-B.; Sun, Z.-Y.; Hu, X.-Q. Mechanical Properties of Steel-FRP Composite Bar under Uniaxial and Cyclic Tensile Loads. J. Mater. Civ. Eng. 2010, 22, 1056–1066. [Google Scholar] [CrossRef]
  37. Wu, G.; Tian, Y. Study on Fabrication Technique of Steel Fiber Composite Bar (SFCB). Earthq. Resist. Eng. Retrofit. 2009, 31, 28–34. [Google Scholar] [CrossRef]
  38. Ding, L.; Lei, M.; Wang, X.; Shi, Y.; Zhu, Z.; Yu, P. Durability of concrete members reinforced with steel-FRP composite bars under dry-wet cycles of seawater. Structures 2021, 33, 2273–2283. [Google Scholar] [CrossRef]
  39. Ge, W.; Han, M.; Guan, Z.; Zhang, P.; Ashour, A.; Li, W.; Lu, W.; Cao, D.; Yao, S. Tension and bonding behaviour of steel-FRP composite bars subjected to the coupling effects of chloride corrosion and load. Constr. Build. Mater. 2021, 296, 123641. [Google Scholar] [CrossRef]
  40. Wu, G.; Wang, X.; Wu, Z.; Dong, Z.; Zhang, G. Durability of basalt fibers and composites in corrosive environments. J. Compos. Mater. 2014, 49, 873–887. [Google Scholar] [CrossRef]
  41. Wu, Z.; Wu, G.; Lv, Z. Earthquake-Resistant Concrete Structures Reinforced by Steel-FRP Composite Bar. 2006. Available online: https://wenku.baidu.com/view/60e9cb84a65177232f60ddccda38376bae1fe0e1?fr=xueshu&_wkts_=1667432958109 (accessed on 2 October 2022). (In Chinese).
  42. Kahl, S.; Jung, J.M.; Wyatt, T.; Atkinson, L.M.; Moser, C.F.; Hayes, M.D.; Steudle, K.T. Stainless and Stainless-Clad Reinforcement for Highway Bridge Use; MDOT OFS Operations Field Services: Lansing, MI, USA, 2012. [Google Scholar]
  43. Cladinox Projects Completed Using Cladinox Author’s Earlier Generation Technology, Produced and Supplied by Stelax UK Ltd. Available online: https://www.cladinox.com/projects (accessed on 31 October 2022).
  44. Cheng, L.; Wu, H.; Li, J.; Zhao, H.; Wang, L. Polydopamine modified ultrathin hydroxyapatite nanosheets for anti-corrosion reinforcement in polymeric coatings. Corros. Sci. 2021, 178, 109064. [Google Scholar] [CrossRef]
  45. Singh, S.; Prakash, C.; Singh, H. Deposition of HA-TiO2 by plasma spray on β-phase Ti-35Nb-7Ta-5Zr alloy for hip stem: Characterization, mechanical properties, corrosion, and in-vitro bioactivity. Surf. Coat. Technol. 2020, 398, 126072. [Google Scholar] [CrossRef]
  46. Liu, D.; Zhao, W.; Liu, S.; Cen, Q.; Xue, Q. Comparative tribological and corrosion resistance properties of epoxy composite coatings reinforced with functionalized fullerene C60 and graphene. Surf. Coat. Technol. 2016, 286, 354–364. [Google Scholar] [CrossRef]
  47. Li, H.; He, Y.; Luo, P.; Fan, Y.; Gou, L.; Li, Z.; Zhao, Y.; Liu, B.; He, T.; Zhang, H. Preparation of laminar α-ZrP nanosheets enhanced NiW nanocomposite coating and investigation of its mechanical and anti-corrosion properties. Surf. Coat. Technol. 2021, 423, 127590. [Google Scholar] [CrossRef]
  48. Ding, R.; Chen, S.; Lv, J.; Zhang, W.; Zhao, X.; Liu, J.; Wang, X.; Gui, T.; Li, B.; Tang, Y.; et al. Study on graphene modified organic anti-corrosion coatings: A comprehensive review. J. Alloys Compd. 2019, 806, 611–635. [Google Scholar] [CrossRef]
  49. Lazorenko, G.; Kasprzhitskii, A.; Nazdracheva, T. Anti-corrosion coatings for protection of steel railway structures exposed to atmospheric environments: A review. Constr. Build. Mater. 2021, 288, 123115. [Google Scholar] [CrossRef]
  50. Sun, Z.; Yi, Z.; Gang, W.U. Research Status of Steel-FRP Composite Bar and Its Reinforced Concrete in Civil Engineering Application; Nanjing Tech University: Nanjing, China, 2021. [Google Scholar]
  51. Lens.org. Patent Analysis. Available online: https://www.lens.org/lens/search/patent/analysis?q=Anti-corrosion&preview=true (accessed on 11 October 2022).
  52. Lens.org. Scholar Analysis. Available online: https://www.lens.org/lens/search/scholar/analysis?q=anti-corrosion&p=0&n=10&s=date_published&d=%2B&f=false&e=false&l=en&authorField=author&dateFilterField=publishedYear&orderBy=%2Bdate_published&patentQueryId=a9079722-fd7e-43d8-96e5-a2f416f3b247&presentat (accessed on 11 October 2022).
  53. Yeomans, S.R. Galvanized Steel Reinforcement: Recent Developments and New Opportunities. In Proceedings of the 5th International Federation for Structural Concrete, Melbourne, Australia, 7–11 October 2018. [Google Scholar]
  54. Hasegawa, K.; Morita, M.; Motoda, S. Effect of Relative Humidity on Crack Growth Mechanism of Hot Dip Galvanized Steel in Atmospheric Environment. ECS Trans. 2017, 80, 609–618. [Google Scholar] [CrossRef]
  55. Wang, Y.; Li, P.; Ning, H. Application of Epoxy-coated Reinforcing Steel in Concrete Structure. Hot Work. Technol. 2010, 133–135. [Google Scholar] [CrossRef]
  56. McDonald, D.B. 5-Corrosion of epoxy-coated steel in concrete. In Corrosion of Steel in Concrete Structures; Poursaee, A., Ed.; Woodhead Publishing: Oxford, UK, 2016; pp. 87–110. ISBN 978-1-78242-381-2. [Google Scholar]
  57. Liu, X.; Feng, G.; Liu, X.; Wang, B.; Zhang, H.; Ma, J. Interface characteristics and properties of a high-strength corrosion-resistant stainless steel clad rebar. Metals 2020, 10, 373. [Google Scholar] [CrossRef] [Green Version]
  58. Mudhaffar, M.A.; Saleh, N.A.; Aassy, A. Influence of Hot Clad Rolling Process Parameters on Life Cycle of Reinforced bar of Stainless Steel Carbon Steel Bars. Procedia Manuf. 2017, 8, 353–360. [Google Scholar] [CrossRef]
  59. Shi, Y.; Luo, Z.; Zhou, X.; Xue, X.; Xiang, Y. Post-fire performance of bonding interface in explosion-welded stainless-clad bimetallic steel. J. Constr. Steel Res. 2022, 193, 107285. [Google Scholar] [CrossRef]
  60. Xiang, Y.; Huang, L.; Zeng, L.; Hu, Y.; Xie, Z. The Future of High Strength Stainless Steel Cladding Bar in Marine Concrete Structures. 2018. Available online: https://kns.cnki.net/KCMS/detail/detail.aspx?dbcode=CPFD&filename=FYHS201812001008 (accessed on 10 May 2022). (In Chinese).
  61. Xu, Y. Research on Basic Properties of Steel Fiber Composite Bars Reinforced Marine Sand Concrete Beams; Southeast University: Nanjing, China, 2015. [Google Scholar]
  62. Ma, G.; Huang, Y.; Aslani, F.; Kim, T. Tensile and bonding behaviours of hybridized BFRP—Steel bars as concrete reinforcement. Constr. Build. Mater. 2019, 201, 62–71. [Google Scholar] [CrossRef]
  63. Wu, G.; Luo, Y.; Wu, Z.; Hu, X.; Zhang, M. Experimental and Theoretical Studies on the Mechanical Properties of steel-FRP Composite Bars. Chin. J. Civ. Eng. 2010, 43, 53–61. [Google Scholar] [CrossRef]
  64. Li, L.; Hou, B.; Lu, Z.; Liu, F. Fatigue behaviour of sea sand concrete beams reinforced with basalt fibre-reinforced polymer bars. Constr. Build. Mater. 2018, 179, 160–171. [Google Scholar] [CrossRef]
  65. Metals, A.S. The Atlas Specialty Metals Technical Handbook of Bar Products; Atlas Specialty Metals: Mowbray, Australia, 2005. [Google Scholar]
  66. Dong, Z.; Wu, G. Research progress on durability of FRP bars reinforced concrete structures. China Civ. Eng. J. 2019, 52, 1–19, 29. [Google Scholar] [CrossRef]
  67. Zinc–Strength–Hardness–Elasticity–Crystal Structure. Available online: https://material-properties.org/ (accessed on 1 May 2022).
  68. GB/T13296; Seamless Stainless Steel Tubes for Boiler and Heat Exchanger. Standardization Administration of China: Beijing, China, 2013.
  69. Li, W.; Wang, Q.; Qu, H.; Xiang, Y.; Li, Z. Mechanical properties of HRB400E/316L stainless steel clad rebar under low-cycle fatigue. Structures 2022, 38, 292–305. [Google Scholar] [CrossRef]
  70. Ismail, M.; Muhammad, B. Corrosion behaviour of dual-phase and galvanized steels in concrete. Anti-Corros. Methods Mater. 2012, 59, 132–138. [Google Scholar] [CrossRef]
  71. Mills, C.; Dymond, B.Z. Anchorage of Epoxy-Coated Rebar Using Chemical Adhesives; Minnesota Department of Transportation: Saint Paul, MN, USA, 2019; Volume 1. [Google Scholar]
  72. Basham, K. Choices in corrosion-resistant rebar. Concr. Constr. 1999, 44, 27–33. [Google Scholar]
  73. Val, D.V.; Stewart, M.G. Life-cycle cost analysis of reinforced concrete structures in marine environments. Struct. Saf. 2003, 25, 343–362. [Google Scholar] [CrossRef]
  74. Hua, J.; Wang, F.; Xiang, Y.; Yang, Z.; Xue, X.; Huang, L.; Wang, N. Mechanical properties of stainless-clad bimetallic steel bars exposed to elevated temperatures. Fire Saf. J. 2022, 127, 103521. [Google Scholar] [CrossRef]
  75. Sun, Z.; Tang, Y.; Luo, Y.; Wu, G.; He, X. Mechanical Properties of Steel-FRP Composite Bars under Tensile and Compressive Loading. Int. J. Polym. Sci. 2017, 2017, 5691278. [Google Scholar] [CrossRef] [Green Version]
  76. Sheng, G.; Gong, S. Investigation of low cycle fatigue behavior of building structural steels under earthquake loading. Acta Metall. Sin. Engl. Lett. 1997, 10, 51. [Google Scholar]
  77. Tang, Y.; Sun, Z.; Wu, G.; Wei, Y. Experimental Study on Cyclic Behavior of SFCBs with Different Slenderness Ratios. J. Mater. Civ. Eng. 2021, 33, 04021204. [Google Scholar] [CrossRef]
  78. Yang, Y.; Wu, G.; Wu, Z.-S. Fatigue Performance of Ballastless Track Slabs Reinforced with BFRP and SFCB. J. Compos. Constr. 2017, 21, 04016069. [Google Scholar] [CrossRef]
  79. Hua, J.; Wang, F.; Xue, X.; Fan, H.; Yan, W. Fatigue properties of bimetallic steel bar: An experimental and numerical study. Eng. Fail. Anal. 2022, 136, 106212. [Google Scholar] [CrossRef]
  80. Wang, F.; Hua, J.; Xue, X.; Ding, Z.; Lyu, Y.; Liu, Q. Low-cycle fatigue performance of bimetallic steel bar considering the effect of inelastic buckling. Constr. Build. Mater. 2022, 351, 128787. [Google Scholar] [CrossRef]
  81. Hua, J.; Yang, Z.; Zhou, F.; Hai, L.; Wang, N.; Wang, F. Effects of exposure temperature on low–cycle fatigue properties of Q690 high–strength steel. J. Constr. Steel Res. 2022, 190, 107159. [Google Scholar] [CrossRef]
  82. Hua, J.; Yang, Z.; Wang, F.; Xue, X.; Wang, N.; Huang, L. Relation between the metallographic structure and mechanical properties of a bimetallic steel bar after fire. J. Mater. Civ. Eng. 2022, 34, 04022193. [Google Scholar] [CrossRef]
  83. Shi, Y.; Luo, Z.; Zhou, X.; Xue, X.; Li, J. Post-fire mechanical properties of titanium–clad bimetallic steel in different cooling approaches. J. Constr. Steel Res. 2022, 191, 107169. [Google Scholar] [CrossRef]
  84. Tariq, F.; Bhargava, P. Residual mechanical behavior of (SD 500) hot rolled TMT reinforcing steel bars after elevated temperatures. Constr. Build. Mater. 2018, 190, 551–559. [Google Scholar] [CrossRef]
  85. Zhong, T.; Xing-Qiang, W.; Brian, U. Stress-Strain Curves of Structural and Reinforcing Steels after Exposure to Elevated Temperatures. J. Mater. Civ. Eng. 2013, 25, 1306–1316. [Google Scholar] [CrossRef]
  86. Gardner, L.; Bu, Y.; Francis, P.; Baddoo, N.R.; Cashell, K.A.; McCann, F. Elevated temperature material properties of stainless steel reinforcing bar. Constr. Build. Mater. 2016, 114, 977–997. [Google Scholar] [CrossRef]
  87. Elghazouli, A.Y.; Cashell, K.A.; Izzuddin, B.A. Experimental evaluation of the mechanical properties of steel reinforcement at elevated temperature. Fire Saf. J. 2009, 44, 909–919. [Google Scholar] [CrossRef] [Green Version]
  88. Chauhan, A.; Hoffmann, J.; Litvinov, D.; Aktaa, J. High-temperature low-cycle fatigue behavior of a 9Cr-ODS steel: Part 2—Hold time influence, microstructural evolution and damage characteristics. Mater. Sci. Eng. A 2018, 730, 197–206. [Google Scholar] [CrossRef]
  89. Cabet, C.; Carroll, L.; Wright, R. Low cycle fatigue and creep-fatigue behavior of alloy 617 at high temperature. J. Press. Vessel Technol. Trans. ASME 2013, 135, 061401. [Google Scholar] [CrossRef]
  90. Hua, J.; Wang, F.; Yang, Z.; Xue, X.; Huang, L.; Chen, Z. Low-cycle fatigue properties of bimetallic steel bars after exposure to elevated temperature. J. Constr. Steel Res. 2021, 187, 106959. [Google Scholar] [CrossRef]
  91. Hua, J.; Wang, F.; Xue, X. Study on fatigue properties of post-fire bimetallic steel bar with different cooling methods. Structures 2022, 40, 633–645. [Google Scholar] [CrossRef]
  92. Hua, J.; Wang, F.; Xue, X.; Ding, Z.; Chen, Z. Residual monotonic mechanical properties of bimetallic steel bar with fatigue damage. J. Build. Eng. 2022, 55, 104703. [Google Scholar] [CrossRef]
  93. Long, X.; Wang, C.; Zhao, P.; Kang, S. Bond strength of steel reinforcement under different loading rates. Constr. Build. Mater. 2020, 238, 117749. [Google Scholar] [CrossRef]
  94. Zhao, D.; Pan, J.; Zhou, Y.; Sui, L.; Ye, Z. New types of steel-FRP composite bar with round steel bar inner core: Mechanical properties and bonding performances in concrete. Constr. Build. Mater. 2020, 242, 118062. [Google Scholar] [CrossRef]
  95. Hamad, B.S.; Mike, J.A. Bond strength of hot-dip galvanized reinforcement in normal strength concrete structures. Constr. Build. Mater. 2005, 19, 275–283. [Google Scholar] [CrossRef]
  96. Kayali, O.; Yeomans, S.R. Bond of ribbed galvanized reinforcing steel in concrete. Cem. Concr. Compos. 2000, 22, 459–467. [Google Scholar] [CrossRef]
  97. Hamad, B.S.; Jumaa, G.K. Bond strength of hot-dip galvanized hooked bars in high strength concrete structures. Constr. Build. Mater. 2008, 22, 2042–2052. [Google Scholar] [CrossRef]
  98. Pokorný, P.; Dobiáš, D.; Vokáč, M. Bond strength of HOT—Dip galvanized reinforcement (B500b) with concrete. Metalurgija 2016, 55, 337–340. [Google Scholar]
  99. Treece, R.A.; Jirsa, J.O. Bond strength of epoxy-coated reinforcing bars. ACI Mater. J. 1989, 86, 167–174. [Google Scholar] [CrossRef]
  100. Assaad, J.J.; Issa, C.A. Bond strength of epoxy-coated bars in underwater concrete. Constr. Build. Mater. 2012, 30, 667–674. [Google Scholar] [CrossRef]
  101. Hua, J.; Yang, Z.; Xue, X.; Huang, L.; Wang, N.; Chen, Z. Bond properties of bimetallic steel bar in seawater sea-sand concrete at different ages. Constr. Build. Mater. 2022, 323, 126539. [Google Scholar] [CrossRef]
  102. Ban, H.; Chen, Z.; Xiang, Y.; Li, Z. Bond behaviour of stainless-clad bimetallic rebar in concrete. Structures 2022, 37, 1069–1079. [Google Scholar] [CrossRef]
  103. Sun, Y.; Sun, Z.; Yao, L.; Wei, Y.; Wu, G. Bond performance between SFCBs and grouted sleeves for precast concrete structures. Adv. Struct. Eng. 2021, 24, 2857–2869. [Google Scholar] [CrossRef]
  104. Han, S.; Fan, C.; Zhou, A.; Ou, J. Simplified implementation of equivalent and ductile performance for steel-FRP composite bars reinforced seawater sea-sand concrete beams: Equal-stiffness design method. Eng. Struct. 2022, 266, 114590. [Google Scholar] [CrossRef]
  105. Huang, Y.; Zhang, Y.; Li, X.; Ying, J. Bond of epoxy-coated steel bars to seawater sea sand recycled concrete. Structures 2021, 30, 866–876. [Google Scholar] [CrossRef]
  106. Almusallam, A.A. Effect of degree of corrosion on the properties of reinforcing steel bars. Constr. Build. Mater. 2001, 15, 361–368. [Google Scholar] [CrossRef]
  107. Chao, C.Y.; Lin, L.F.; Macdonald, D.D. A Point Defect Model for Anodic Passive Films: I. Film Growth Kinetics. J. Electrochem. Soc. 1981, 128, 1187–1194. [Google Scholar] [CrossRef]
  108. Apostolopoulos, C.A.; Papadakis, V.G. Consequences of steel corrosion on the ductility properties of reinforcement bar. Constr. Build. Mater. 2008, 22, 2316–2324. [Google Scholar] [CrossRef]
  109. Griffith, A.; Laylor, H.M. Epoxy Coated Final Report. 1999. Available online: https://rosap.ntl.bts.gov/view/dot/14421 (accessed on 10 May 2022).
  110. Brown, M.C. Corrosion Protection Service Life of Epoxy Coated Reinforcing; Virginia Polytechnic Institute: Blacksburg, VA, USA, 2002. [Google Scholar]
  111. Tahri, W.; Hu, X.; Shi, C.; Zhang, Z. Review on corrosion of steel reinforcement in alkali-activated concretes in chloride-containing environments. Constr. Build. Mater. 2021, 293, 123484. [Google Scholar] [CrossRef]
  112. Robertson, J. The mechanism of high temperature aqueous corrosion of stainless steels. Corros. Sci. 1991, 32, 443–465. [Google Scholar] [CrossRef]
  113. Martin, U.; Ress, J.; Bosch, J.; Bastidas, D.M. Stress corrosion cracking mechanism of AISI 316LN stainless steel rebars in chloride contaminated concrete pore solution using the slow strain rate technique. Electrochim. Acta 2020, 335, 135565. [Google Scholar] [CrossRef]
  114. Moser, R.D.; Singh, P.M.; Kahn, L.F.; Kurtis, K.E.; Niño, D.G.; McClelland, Z.B. Crevice corrosion and environmentally assisted cracking of high-strength duplex stainless steels in simulated concrete pore solutions. Constr. Build. Mater. 2019, 203, 366–376. [Google Scholar] [CrossRef]
  115. Saeki, I.; Ohno, T.; Seto, D.; Sakai, O.; Sugiyama, Y.; Sato, T.; Yamauchi, A.; Kurokawa, K.; Takeda, M.; Onishi, T. Measurement of Young’s modulus of oxides at high temperature related to the oxidation study. Mater. High Temp. 2011, 28, 264–268. [Google Scholar] [CrossRef]
  116. Clear, K.C. Effectiveness of Epoxy-Coated Reinforcing Steel-Final Report; Canadian Strategic Highway Research Program: Ottawa, ON, Canada, 1992. [Google Scholar]
  117. Cui, M.; Ren, S.; Zhao, H.; Xue, Q.; Wang, L. Polydopamine coated graphene oxide for anticorrosive reinforcement of water-borne epoxy coating. Chem. Eng. J. 2018, 335, 255–266. [Google Scholar] [CrossRef]
  118. Zheng, W.; Chen, W.G.; Feng, T.; Li, W.Q.; Liu, X.T.; Dong, L.L.; Fu, Y.Q. Enhancing chloride ion penetration resistance into concrete by using graphene oxide reinforced waterborne epoxy coating. Prog. Org. Coat. 2020, 138, 105389. [Google Scholar] [CrossRef]
  119. Zhu, Q.; Li, E.; Liu, X.; Song, W.; Li, Y.; Wang, X.; Liu, C. Epoxy coating with in-situ synthesis of polypyrrole functionalized graphene oxide for enhanced anticorrosive performance. Prog. Org. Coat. 2020, 140, 105488. [Google Scholar] [CrossRef]
  120. Zhu, Q.; Zhang, K.; Huang, Y.; Liu, R.; Pan, Y.; Zhang, H.; Wang, P.; Zhang, S.; Pan, D.; Guo, Z. Hydrothermally synthesized ZnO-reduced graphene oxide nanocomposite for enhanced anticorrosion performance of waterborne epoxy coating. J. Nanostruct. Chem. 2022, 12, 277–289. [Google Scholar] [CrossRef]
  121. Nkurunziza, G.; Debaiky, A.; Cousin, P.; Benmokrane, B. Durability of GFRP bars: A critical review of the literature. Prog. Struct. Eng. Mater. 2005, 7, 194–209. [Google Scholar] [CrossRef]
  122. Jungkuist, D.A. Simulation of Enviro-Mechanical Durability for Life Prediction of E-Glass/Vinyl Ester Composites Using a Bridge Service Environment; Virginia Tech: Blacksburg, VA, USA, 2000. [Google Scholar]
  123. Feng, G.; Zhu, D.; Guo, S.; Rahman, M.Z.; Jin, Z.; Shi, C. A review on mechanical properties and deterioration mechanisms of FRP bars under severe environmental and loading conditions. Cem. Concr. 2022, 134, 104758. [Google Scholar] [CrossRef]
  124. Li, Z.; Xiao, T.; Zhao, S. Effects of surface treatments on Mechanical properties of Continuous basalt fibre cords and their Adhesion with rubber matrix. Fibers Polym. 2016, 17, 910–916. [Google Scholar] [CrossRef]
  125. SHRP2. Chloride Threshold for Various Reinforcement Steel Types Reinforcement Steel Types, n.d. Available online: http://shrp2.transportation.org/documents/Appendix_C-Chloride_threshold_v3.pdf (accessed on 2 May 2022).
  126. Darwin, D.; Browning, J.; O’Reilly, M.; Xing, L.; Ji, J. Critical chloride corrosion threshold of galvanized reinforcing bars. ACI Mater. J. 2009, 106, 176–183. [Google Scholar] [CrossRef]
  127. Lawler, J.S.; Kurth, J.C.; Garrett, S.M.; Krauss, P.D. Statistical distributions for chloride thresholds of reinforcing bars. ACI Mater. J. 2021, 118, 13–20. [Google Scholar] [CrossRef]
  128. Tsutsumi, Y.; Nishikata, A.; Tsuru, T. Pitting corrosion mechanism of Type 304 stainless steel under a droplet of chloride solutions. Corros. Sci. 2007, 49, 1394–1407. [Google Scholar] [CrossRef]
  129. Xu, G.; Zhang, D.; Liu, D.; Wei, J. Research on mechanical properties of corroded steel bar in concrete under chloride environment. J. Hydraul. 2012, 43, 452–459. [Google Scholar] [CrossRef]
  130. Apostolopoulos, C.A.; Papadopoulos, M.P.; Pantelakis, S.G. Tensile behavior of corroded reinforcing steel bars BSt 500s. Constr. Build. Mater. 2006, 20, 782–789. [Google Scholar] [CrossRef]
  131. Zhang, W.; Song, X.; Gu, X.; Li, S. Tensile and fatigue behavior of corroded rebars. Constr. Build. Mater. 2012, 34, 409–417. [Google Scholar] [CrossRef]
  132. Apostolopoulos, C.A.; Papadopoulos, M.P. Tensile and low cycle fatigue behavior of corroded reinforcing steel bars S400. Constr. Build. Mater. 2007, 21, 855–864. [Google Scholar] [CrossRef]
  133. Gao, P. Study on Mechanical Properties of Sfcb and Its Bond with Concrete under the Coupling of Chloride Salt Erosion and Load; Yangzhou University: Yangzhou, China, 2020. [Google Scholar]
  134. Hua, J.; Fan, H.; Xue, X.; Wang, F.; Chen, Z.; Huang, L.; Wang, N. Tensile and low-cycle fatigue performance of bimetallic steel bars with corrosion. J. Build. Eng. 2021, 43, 103188. [Google Scholar] [CrossRef]
  135. Miyazato, S.; Nakazawa, R. Evaluation of Corrosion and Tensile Strength of Epoxy Coated Rebar with Damage in Mortar. Cem. Sci. Concr. Technol. 2015, 69, 387–394. [Google Scholar] [CrossRef] [Green Version]
  136. Zhou, Y.; Zheng, X.; Xing, F.; Sui, L.; Zheng, Y.; Huang, X. Investigation on the electrochemical and mechanical performance of CFRP and steel-fiber composite bar used for impressed current cathodic protection anode. Constr. Build. Mater. 2020, 255, 119377. [Google Scholar] [CrossRef]
  137. Zhou, Y.; Zheng, Y.; Pan, J.; Sui, L.; Xing, F.; Sun, H.; Li, P. Experimental investigations on corrosion resistance of innovative steel-FRP composite bars using X-ray microcomputed tomography. Compos. Part B Eng. 2019, 161, 272–284. [Google Scholar] [CrossRef]
  138. Hua, J.; Wang, F.; Wang, N.; Huang, L.; Hai, L.; Li, Y.; Zhu, X.; Xue, X. Experimental and numerical investigations on corroded stainless-clad bimetallic steel bar with artificial damage. J. Build. Eng. 2021, 44, 102779. [Google Scholar] [CrossRef]
  139. Hua, J.; Fan, H.; Yan, W.; Wang, N.; Xue, X.; Huang, L. Seismic resistance of the corroded bimetallic steel bar under different strain amplitudes. Constr. Build. Mater. 2022, 319, 126088. [Google Scholar] [CrossRef]
  140. Wang, X.H.; Gao, Y. Corrosion behavior of epoxy-coated reinforced bars in RC test specimens subjected to pre-exposure loading and wetting-drying cycles. Constr. Build. Mater. 2016, 119, 185–205. [Google Scholar] [CrossRef]
  141. Huang, Y.; Qi, X.; Li, C.; Gao, P.; Wang, Z.; Ying, J. Seismic behaviour of seawater coral aggregate concrete columns reinforced with epoxy-coated bars. Structures 2022, 36, 822–836. [Google Scholar] [CrossRef]
  142. Caraguay, S.J.; Pereira, T.S.; Giacomelli, R.O.; Cunha, A.; Pereira, M.; Xavier, F.A. The effect of laser surface textures on the corrosion resistance of epoxy coated steel exposed to aggressive environments for offshore applications. Surf. Coat. Technol. 2022, 437, 128371. [Google Scholar] [CrossRef]
  143. Shuo, D.; Yuanming, D. Study on Static and Fatigue Performance Test for Corrosion Resistant Reinforced Concrete Beam; Hebei University of Technology: Tianjin, China, 2016. [Google Scholar]
  144. Fadl, A.M.; Abdou, M.I.; Al-Elaa, S.A.; Hamza, M.A.; Sadeek, S.A. Evaluation the anti-corrosion behavior, impact resistance, acids and alkali immovability of nonylphenol ethoxylate/TiO2 hybrid epoxy nanocomposite coating applied on the carbon steel surface. Prog. Org. Coat. 2019, 136, 105263. [Google Scholar] [CrossRef]
  145. Kim, C.; Goldsberry, R.; Karayan, A.I.; Milla, J.; Goehring, L.; Hassan, M.; Castaneda, H. Electrochemical evaluation of epoxy-coated-rebar containing pH-responsive nanocapsules in simulated carbonated concrete pore solution. Prog. Org. Coat. 2021, 161, 106549. [Google Scholar] [CrossRef]
  146. Cheng, A.; Huang, R.; Wu, J.K.; Chen, C.H. Effect of rebar coating on corrosion resistance and bond strength of reinforced concrete. Constr. Build. Mater. 2005, 19, 404–412. [Google Scholar] [CrossRef]
  147. Andrade, C.; Arteaga, A.; Lopez-Hombrados, C.; Vazquez, A. Tests on Bond of Galvanized Rebar and Concrete Cured in Seawater. J. Mater. Civ. Eng. 2001, 13, 319–324. [Google Scholar] [CrossRef]
  148. Kobayashi, K.; Takewaka, K. Experimental studies on epoxy coated reinforcing steel for corrosion protection. Int. J. Cem. Compos. Lightweight Concr. 1984, 6, 99–116. [Google Scholar] [CrossRef]
  149. El-Hawary, M.M. Evaluation of bond strength of epoxy-coated bars in concrete exposed to marine environment. Constr. Build. Mater. 1999, 13, 357–362. [Google Scholar] [CrossRef]
  150. Dong, Z.; Wu, G.; Xu, Y. Experimental study on the bond durability between steel-FRP composite bars (SFCBs) and sea sand concrete in ocean environment. Constr. Build. Mater. 2016, 115, 277–284. [Google Scholar] [CrossRef]
  151. Dong, Z.; Wu, G.; Zhao, X.L.; Zhu, H.; Lian, J. Bond durability of steel-FRP composite bars embedded in seawater sea-sand concrete under constant bending and shearing stress. Constr. Build. Mater. 2018, 192, 808–817. [Google Scholar] [CrossRef]
  152. Clemena, G.G.; Kukreja, D.N.; Napier, C.S. Trial Use of a Stainless Steel-Clad Steel Bar in a New Concrete Bridge Deck in Virginia; Virginia Transportation Research Council: Charlottesville, VA, USA, 2003; p. 30. Available online: https://rosap.ntl.bts.gov/view/dot/19617 (accessed on 15 May 2022).
  153. Liu, G.; Hua, J.; Wang, N.; Deng, W.; Xue, X. Material Alternatives for Concrete Structures on Remote Islands: Based on Life-cycle cost Analysis. Adv. Civ. Eng. 2022, 2022, 7329408. [Google Scholar] [CrossRef]
  154. Li, J. SCBSB Using in a Bay Bridge. Available online: http://m.ldnews.cn/pcarticle/659574?mobile (accessed on 15 May 2022).
  155. International Zinc Association. Galvanized Rebar Projects. 2022. Available online: https://www.galvanizedrebar.com/project/ (accessed on 15 May 2022).
  156. Zintel, M.; Angst, U.; Keßler, S.; Gehlen, C. Epoxidharzbeschichtete Bewehrung: Neue Erkenntnisse nach zwei Jahrzehnten Praxiserfahrung. Beton- und Stahlbetonbau 2014, 109, 3–14. [Google Scholar] [CrossRef]
  157. Zhang, H.Q. Epoxy Resin Coated Steel Bar Construction Supervision in Shantou LPG Wharf Engineering. PORT Waterw. Eng. 1999, 4, 63–65, 67. [Google Scholar] [CrossRef]
  158. Xu, F. Application of epoxy-coated reinforcing steel in Bachimen Bridge Project. Highway 2002, 2, 783–785. [Google Scholar]
  159. Epoxy Interes Group. Epoxy Projects. 2022. Available online: http://www.epoxyinterestgroup.org/projects/ (accessed on 15 May 2022).
Table 6. Experiments on corroded fatigue properties of GR and SCR.
Table 6. Experiments on corroded fatigue properties of GR and SCR.
RefTypeVariableRemarks
Hasegawa et al., 2017 [54]GRHumidity;
Loading cycles
The humidity has a neglectable effect on the low cycle fatigue performance of galvanized reinforcements.
When the number of cycles to fatigue exceeds 104, the high humidity causes a reduction of fatigue strength.
After failure, cracks on the interface were observed.
Hua et al., 2022 [139]SCRCorrosion degree; strain amplitudesWith the increase of corrosion degree and fatigue strain amplitude, the cycles of fatigue and total energy dissipation reduce.
In the fatigue test, the deformation of stainless steel cladding and steel core are harmonious; no debonding was observed even in severe corrosion.
Note: galvanized reinforcement (GR); stainless cladding reinforcement (SCR).
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Yan, L.; Deng, W.; Wang, N.; Xue, X.; Hua, J.; Chen, Z. Anti-Corrosion Reinforcements Using Coating Technologies—A Review. Polymers 2022, 14, 4782. https://doi.org/10.3390/polym14214782

AMA Style

Yan L, Deng W, Wang N, Xue X, Hua J, Chen Z. Anti-Corrosion Reinforcements Using Coating Technologies—A Review. Polymers. 2022; 14(21):4782. https://doi.org/10.3390/polym14214782

Chicago/Turabian Style

Yan, Lei, Wenjie Deng, Neng Wang, Xuanyi Xue, Jianmin Hua, and Zengshun Chen. 2022. "Anti-Corrosion Reinforcements Using Coating Technologies—A Review" Polymers 14, no. 21: 4782. https://doi.org/10.3390/polym14214782

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop